Study guide
1.3 Mechanical & Non-Destructive Testing of Metals
EASA Part-66 Module 06 — Materials and Hardware Exam
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Ferrous Aircraft Materials
1.1 Alloy Steels, Crystal Structure & Specifications 1.2 Heat Treatment of Ferrous Metals 1.3 Mechanical & Non-Destructive Testing of Metals 1.4 Repair & Inspection Procedures for Ferrous Structures
2 Chapter 2: Non-Ferrous Aircraft Materials
2.1 Aluminium & Aluminium Alloy Classifications 2.2 Heat Treatment & Temper Designations of Aluminium 2.3 Titanium, Magnesium & High-Temperature Alloys 2.4 Repair & Inspection Procedures for Non-Ferrous Structures
3 Chapter 3: Composite and Non-Metallic Materials
3.1 Composite Fibres, Resins & Core Materials 3.2 Sandwich Construction, Damage Modes & Repair 3.3 Wood, Fabric, Plastics & Sealants 3.4 Wooden Structures: Construction, Preservation & Repair 3.5 Fabric Covering: Inspection, Defects & Repair
4 Chapter 4: Aircraft Corrosion & Surface Protection
4.1 Principles & Chemical Fundamentals of Corrosion 4.2 Forms & Mechanisms of Aircraft Corrosion 4.3 Corrosion Inspection, Removal & Protective Treatments
5 Chapter 5: Fasteners — Threaded Fasteners & Locking Devices
5.1 Screw Threads & Thread Specifications 5.2 Aircraft Bolts, Screws & Studs 5.3 Locking Devices, Safety Wiring & Torque Procedures 5.4 Anchor Nuts, Self-Tapping Screws & Dowels 5.5 Quick-Release Fasteners, Circlips & Keys
6 Chapter 6: Fasteners — Aircraft Rivets
6.1 Solid Aircraft Rivets & Installation Practice 6.2 Blind Fasteners, Structural Fasteners & Inspection
7 Chapter 7: Pipes, Flexible Hoses & Unions
7.1 Aircraft Rigid Tubing Materials & Fabrication 7.2 Flexible Hoses & Fluid Line Identification 7.3 Aircraft Pipe Unions, Fittings & Installation
8 Chapter 8: Springs
8.1 Types, Materials & Mechanics of Aircraft Springs 8.2 Spring Testing, Inspection & Failure Modes
9 Chapter 9: Bearings
9.1 Plain Bearings, Bushings & Spherical Bearings 9.2 Rolling-Element Bearings: Ball & Roller Types 9.3 Bearing Handling, Lubrication & Defect Analysis
10 Chapter 10: Transmissions & Mechanical Drives
10.1 Gear Types, Geometries & Epicyclic Systems 10.2 Gear Ratios, Mesh Alignment, Belts & Chains
11 Chapter 11: Flight Control Cables
11.1 Aircraft Control Cable Construction & Sizing 11.2 Cable End Fittings, Swaging & Turnbuckles 11.3 Pulleys, Rigging, Tension Regulators & Cable Maintenance
12 Chapter 12: Electrical Cables & Connectors (EWIS)
12.1 EWIS Conductor Types, Insulation & AWG Sizing 12.2 Wire Harness Bundling, Routing & Clamping 12.3 Connectors, Crimping Practice & Contact Assembly 12.4 High-Tension Ignition Cables & Coaxial Transmission Lines
1.3 Mechanical & Non-Destructive Testing of Metals
Key Takeaways Explain This Topic AI
Tensile testing establishes fundamental engineering properties: Young's modulus of elasticity (~205 GPa for steels), 0.2% proof stress (yield strength), ultimate tensile strength (UTS), and ductility (% elongation and reduction of area).
Rockwell C hardness testing utilizes a 120° diamond spheroconical Brale indenter under 150 kgf total load for hardened steels, whereas Brinell hardness testing applies a 10 mm ball under 3000 kgf load, yielding an approximate tensile strength relationship of UTS (psi) ≈ 500 × BHN.
Charpy V-notch impact testing measures absorbed fracture energy and reveals the Ductile-to-Brittle Transition Temperature (DBTT) characteristic of BCC ferrous steels, a critical factor for high-altitude aircraft operating at -55°C that does not occur in FCC austenitic alloys.
Ferrous steels exhibit a distinct fatigue limit (endurance limit) on an S-N curve (~40%–50% of UTS) below which cyclic stresses will never cause fatigue failure, unlike non-ferrous alloys which lack a true endurance limit.
Magnetic Particle Inspection (MPI) detects surface and near-subsurface flaws exclusively in ferromagnetic materials; longitudinal coil magnetization detects transverse flaws, circular magnetization detects longitudinal flaws, and post-inspection demagnetization (< 3 Gauss) is strictly mandatory.
Last updated: September 2026
1.3 Mechanical & Non-Destructive Testing of Metals
Airworthiness certification and continuing airworthiness management require quantitative verification of material integrity. Testing divides into two fundamental branches: Destructive Mechanical Testing , in which standardized test specimens are loaded to failure to establish baseline design properties, and Non-Destructive Testing (NDT) , where operational aircraft components are inspected for defects without impairing their future serviceability.
Under EASA Part-66 Module 06 , technicians must be proficient in interpreting tensile curves, hardness scales, impact energy data, fatigue mechanisms, and NDT inspection principles.
Destructive Mechanical Testing: The Tensile Test
The tensile test (conducted per ASTM E8 or EN ISO 6892) measures the response of a metal to uniaxial tensile loading. A standardized machined "dog-bone" specimen with original gauge length ( L 0 L_0 L 0 ) and cross-sectional area ( A 0 A_0 A 0 ) is pulled at a controlled strain rate until fracture. Stress (σ) [MPa]
- ^
- UTS | * Peak (Ultimate Tensile Strength, Rm)
- (Rm) | / \
- | / \ Necking begins
- Re/ | * Yield Point (Rp0.2 / 0.2% Offset)
- Rp0.2| / \
- | / * Fracture (Ru)
- | / Elastic |
- | / Region | Plastic Deformation Region
- | / |
- | / Hooke's Law |
- |---* Proportional |
- | | Limit (σ = E·ε)|
- └───┴────────────────┴───────────────────────> Strain (ε) [mm/mm]
- 0.002 (0.2% Offset)
- Stress-Strain Terminology and Parameters
Engineering Stress ( σ \sigma σ ) : Applied load ( P P P ) divided by the original cross-sectional area ( A 0 A_0 A 0 ): σ = P A 0 [ MPa or psi ] \sigma = \frac{P}{A_0} \quad [\text{MPa or psi}] σ = A 0 P [ MPa or psi ]
Engineering Strain ( ϵ \epsilon ϵ ) : Elongation ( Δ L = L − L 0 \Delta L = L - L_0 Δ L = L − L 0 ) divided by the original gauge length ( L 0 L_0 L 0 ): ϵ = L − L 0 L 0 = Δ L L 0 [ dimensionless or % ] \epsilon = \frac{L - L_0}{L_0} = \frac{\Delta L}{L_0} \quad [\text{dimensionless or } \%] ϵ = L 0 L − L 0 = L 0 Δ L [ dimensionless or % ]
Modulus of Elasticity (Young's Modulus, E E E ) : The slope of the linear elastic portion of the stress-strain curve where Hooke's Law applies ( σ = E ⋅ ϵ \sigma = E \cdot \epsilon σ = E ⋅ ϵ ). For virtually all aircraft steels, Young's modulus is approximately 205 to 210 GPa ( 30 × 10 6 psi 30 \times 10^6\text{ psi} 30 × 1 0 6 psi ) , irrespective of whether the steel is annealed, normalised, or heat-treated to maximum hardness.
Proportional Limit and Elastic Limit : The highest stress at which stress remains directly proportional to strain (proportional limit), and the maximum stress a material can withstand without permanent plastic deformation upon unloading (elastic limit).
Yield Strength / 0.2% Proof Stress ( R p 0.2 R_{p0.2} R p 0.2 ) : Most high-strength alloy steels do not display a sharp, distinct yield point drop. Instead, yield strength is measured using the 0.2% offset method : a line is drawn parallel to the linear elastic slope starting at a strain of 0.002 (0.2%) . The stress where this line intersects the stress-strain curve is designated the 0.2% Proof Stress ( R p 0.2 R_{p0.2} R p 0.2 ) .
Ultimate Tensile Strength (UTS, R m R_m R m ) : The maximum engineering stress sustained by the specimen before localized cross-sectional thinning ( necking ) begins.
Ductility Measures :
Percentage Elongation (% EL) : Measures overall plastic tensile stretch: % EL = ( L f − L 0 L 0 ) × 100 \%\text{EL} = \left( \frac{L_f - L_0}{L_0} \right) \times 100 % EL = ( L 0 L f − L 0 ) × 100
Percentage Reduction of Area (% RA) : Measures localized necking capability: % RA = ( A 0 − A f A 0 ) × 100 \%\text{RA} = \left( \frac{A_0 - A_f}{A_0} \right) \times 100 % RA = ( A 0 A 0 − A f ) × 100
Hardness Testing of Ferrous Metals
Hardness is defined as the resistance of a material to localized plastic deformation, penetration, or scratching. Because hardness correlates directly with ultimate tensile strength, it serves as the most widely used quality control inspection in aircraft maintenance.
Test Method Indenter Geometry Applied Test Load Measurement Principle Aircraft Application & Limitations
Brinell (HBW) 10 mm hardened tungsten carbide ball 3000 kgf (for steel; 500 kgf for soft metals) for 10–15 s Optical diameter ( d d d ) of residual spherical indentation Heavy forgings, castings; cannot test thin sheets or case-hardened layers; indentation too large for finished parts
Rockwell C (HRC) 120° spheroconical diamond Brale 150 kgf total (10 kgf minor preload + 140 kgf major load) Differential depth of penetration read directly on dial/screen Hardened alloy steels ( SAE 4130, 4340, 300M ), landing gear bolts (> 1000 MPa UTS); valid 20 to 70 HRC
Rockwell B (HRB) 1/16-inch (1.588 mm) tungsten carbide ball 100 kgf total (10 kgf minor preload + 90 kgf major load) Differential depth of penetration read directly on dial/screen Annealed alloy steels, normalized sheet, aluminum alloys, brass; valid 0 to 100 HRB
Vickers (HV) 136° square-based diamond pyramid 1 kgf to 120 kgf Optical average of two indentation diagonal lengths ( d 1 , d 2 d_1, d_2 d 1 , d 2 ) Universal continuous scale from soft aluminum to hardest nitrided layers; precision laboratory testing
Knoop (HK) Rhombic-based pyramidal diamond (7:1 diagonal ratio) Micro-loads: 1 gf to 1000 gf Optical length of long diagonal Microhardness: thin electroplating (cadmium, chrome), nitrided case depth profiles, individual metallurgical phases
Rockwell Hardness Testing Principles
The Rockwell test is the standard workshop test because it measures the differential depth of penetration , eliminating optical measurement errors and providing an immediate digital readout. The sequence is strictly standardized:
Apply minor load of 10 kgf : Seats the indenter through surface oxides and paint remnants into virgin metal, establishing the zero reference datum plane.
Apply major load (e.g., additional 140 kgf for HRC, bringing total load to 150 kgf): Causes plastic indentation.
Release major load back to minor load (10 kgf) : The instrument measures the permanent increment in indentation depth ( e e e ), displaying the hardness number directly.
Correlation Between Hardness and Tensile Strength
For carbon and low-alloy steels (such as SAE 4130 and 4340), there is a direct empirical relationship between Brinell hardness and ultimate tensile strength: UTS (psi) ≈ 500 × BHN \text{UTS (psi)} \approx 500 \times \text{BHN} UTS (psi) ≈ 500 × BHN UTS (MPa) ≈ 3.45 × BHN \text{UTS (MPa)} \approx 3.45 \times \text{BHN} UTS (MPa) ≈ 3.45 × BHN
Example: An SAE 4340 component testing at 300 BHN has an approximate ultimate tensile strength of 300 × 500 = 150 , 000 psi 300 \times 500 = 150,000\text{ psi} 300 × 500 = 150 , 000 psi (approx. 1035 MPa).
Impact Testing & Ductile-to-Brittle Transition
Impact testing evaluates a material's notch toughness —its capacity to absorb mechanical energy during sudden, high-velocity dynamic fracture in the presence of a sharp stress concentration.
Charpy V-Notch vs. Izod
Charpy V-Notch (ASTM E23 / ISO 148) : The standard test piece (10 mm × 10 mm × 55 mm with a 2 mm deep 45° V-notch) is supported horizontally at both ends as a simple beam . A heavy pendulum hammer is released from height h 1 h_1 h 1 and strikes the specimen directly behind the notch. The hammer fractures the specimen and swings up to height h 2 h_2 h 2 . The energy absorbed by the fracture (in Joules or ft-lb) is calculated from the height difference.
Izod Test : The specimen is clamped vertically as a cantilever beam and struck by the pendulum on the notched face above the clamp.
Ductile-to-Brittle Transition Temperature (DBTT)
When impact specimens of Body-Centered Cubic (BCC) metals (such as carbon steels, low-alloy 4130/4340, and ferritic/martensitic stainless steels) are tested across a range of temperatures, they exhibit a sudden, dramatic drop in energy absorption over a narrow temperature band known as the Ductile-to-Brittle Transition Temperature (DBTT) .
Above DBTT : The fracture surface is dull, fibrous, and displays shear lips (ductile microvoid coalescence, absorbing high energy, e.g., 60–100 J).
Below DBTT : The fracture is bright, highly reflective, crystalline, and flat (brittle cleavage along crystallographic planes, absorbing very low energy, e.g., < 10 J).
Critical Aviation Rule: Commercial jet aircraft cruise at altitudes of 35,000 to 43,000 feet where ambient outside air temperatures reach -55°C to -60°C (-67°F to -76°F) . Any ferrous alloy used in external structures must have its DBTT well below -65°C to prevent catastrophic brittle shatter during landing impacts. Crucially, Face-Centered Cubic (FCC) metals (austenitic stainless steels 304/316/321, aluminum alloys, titanium) DO NOT exhibit a DBTT ; they maintain high toughness and ductility even at cryogenic temperatures (-196°C).
Fatigue Testing and the S-N Curve
Fatigue is the progressive, localized structural damage that occurs when a component is subjected to fluctuating cyclic stresses well below its static tensile yield strength. Fatigue accounts for more than 80% of all in-service mechanical failures in aircraft structures.
The S-N Curve (Wöhler Diagram)
Fatigue performance is mapped by testing specimens at various cyclic stress amplitudes ( S S S ) and recording the number of cycles to failure ( N N N , plotted on a logarithmic scale). Cyclic Stress Amplitude (S)
- ^
- |
- | * (High Stress - Low Cycle Fatigue)
- | \
- | \ Aluminium / Non-Ferrous (No Fatigue Limit)
- | \ *-------------------
- | \ \
- | \ \
- Se |---------*============\======================== Ferrous Steels (True Fatigue Limit, Se)
- | \ \
- | \ *
- └────────────┴────────────┴─────────────────────> Cycles to Failure (N, log scale)
- 10^6 10^7
- Ferrous Endurance Limit vs. Non-Ferrous Alloys
Ferrous Metals (Steels) : Display a distinct horizontal asymptote on the S-N curve known as the Fatigue Limit (or Endurance Limit, S e S_e S e ) , typically occurring between 10 6 10^6 1 0 6 and 10 7 10^7 1 0 7 cycles. For polished steel specimens, S e S_e S e is approximately 40% to 50% of the Ultimate Tensile Strength (UTS) . If cyclic stress amplitudes remain below this endurance limit, the component can theoretically withstand an infinite number of cycles without failing.
Non-Ferrous Alloys (Aluminium, Titanium, Copper) : Do not possess a true fatigue limit . Their S-N curves continue to slope downward indefinitely. For non-ferrous parts, engineers must define fatigue strength at a specific design life (e.g., 10 7 10^7 1 0 7 or 10 8 10^8 1 0 8 cycles).
Morphology of Fatigue Failure
Examining an aircraft fatigue fracture under magnification reveals three distinct zones:
Crack Initiation Site : Typically at a surface stress concentration (sharp radius, corrosion pit, tool score mark, inclusion).
Fatigue Crack Propagation Area : Characterized by smooth, burnished surfaces displaying concentric "beach marks" (clamshell arrest marks) that represent the progressive advance of the crack front during successive flight cycles.
Fast Fracture Overload Zone : The final remaining cross-section suddenly fails in static overload (coarse, dull ductile shear or bright brittle cleavage) when it can no longer support the operating load.
Non-Destructive Testing (NDT) of Aircraft Ferrous Hardware
Non-Destructive Testing allows maintenance engineers to inspect parts for crack initiation, corrosion, manufacturing defects, and structural degradation without compromising future airworthiness.
1. Magnetic Particle Inspection (MPI)
Magnetic Particle Inspection is the premier NDT method for detecting surface and near-subsurface discontinuities in ferromagnetic materials (carbon steels, alloy steels 4130/4340, and 400-series martensitic stainless steels).
Exam Warning / Common Trap: MPI CANNOT be performed on austenitic stainless steels (AISI 300 series) such as 304, 316, 321, or 347. Austenitic stainless steels have an FCC crystal structure and are non-magnetic ; they cannot sustain magnetic flux fields.
Operational Principle
When a ferromagnetic part is magnetized, magnetic lines of force (flux lines) pass through the material. If a surface or near-surface crack interrupts these flux lines, the flux cannot jump the air gap easily. Instead, it detours around the defect, with some lines leaking out into the air above the crack, creating localized North and South magnetic poles ( magnetic flux leakage field ). When fine ferromagnetic oxide particles (colored or fluorescent) are applied, they are magnetically drawn to the leakage field, forming a sharp, visible indication.
Magnetization Techniques
Circular Magnetization : Created by passing high-amperage current directly through the component (via headstock contact clamps) or through a central copper conductor bar placed through a hollow bore. The magnetic field circles around the part circumference. Because flux lines must cut across defects at approximately 90° (minimum 45°) to create leakage fields, circular magnetization detects longitudinal cracks parallel to the axis .
Longitudinal Magnetization : Created by placing the component inside an encircling solenoid coil or wrapping a flexible current-carrying cable around it. The magnetic flux flows parallel to the longitudinal axis. Longitudinal magnetization detects transverse and circumferential cracks perpendicular to the axis .
Current Types and Application Methods
Alternating Current (AC) : Subject to the "skin effect," which concentrates magnetic flux in the outer 1 mm to 2 mm of the surface. Provides maximum sensitivity for fine surface fatigue cracks .
Direct Current (DC) / Half-Wave Rectified (HWDC) : Penetrates deeper into the cross-section, providing superior detection of near-subsurface flaws (such as subsurface forging inclusions).
Continuous Method : Magnetic particle suspension is sprayed over the part while the magnetizing current pulse is actively energized. Mandatory for aircraft steels with low magnetic retentivity.
Residual Method : Particles are applied after the magnetizing current has been shut off, relying on residual magnetism. Permissible only for high-retentivity, fully hardened steels.
Demagnetization
Following MPI, components retain residual magnetism, which would attract abrasive ferrous wear particles, freeze up instruments, cause electric arcing in bearings, and severely deflect the aircraft's primary magnetic compasses. Demagnetization is mandatory . It is performed by passing the component through an AC demagnetizing coil and slowly withdrawing it along the coil axis for at least 1.5 meters, or using decreasing step-down reversing DC current. The component must be checked with a calibrated field indicator (Gauss meter) to verify residual field is below 2 to 3 Gauss .
2. Overview of Complementary Aviation NDT Methods
NDT Method Operating Physics Materials Inspectable Defect Capabilities Aircraft Applications & Limitations
Fluorescent Penetrant (FPI) Capillary action draws low-surface-tension fluorescent liquid dye into surface openings; developer draws dye back out; viewed under UV-A (365 nm) Any non-porous solid (Austenitic CRES, aluminum, titanium, ceramics, unmagnetized parts) Surface-breaking flaws ONLY ; cannot detect subsurface flaws Turbine blades, fittings, austenitic exhaust manifolds; surface must be chemically clean; paint must be completely stripped
Eddy Current Testing (ECT) High-frequency AC coil induces circular eddy currents in conductive material; cracks disrupt eddy currents, altering coil impedance Any electrically conductive metal (ferrous and non-ferrous) Surface and near-surface cracks; conductivity changes; coating thickness Bolt-hole inspections in wing spars, wheel halves; can inspect through paint and non-conductive primers ; sensitive to edge effects
Ultrasonic Testing (UT) High-frequency acoustic sound waves (0.5 to 15 MHz) pulsed into part via piezoelectric transducer with couplant gel; echoes reflected back All metals, composites, plastics Internal volumetric voids, laminations, forging bursts, wall thickness thinning Landing gear shock strut wall thickness, internal delaminations in composite-to-steel joints; requires liquid couplant; geometry-sensitive
Radiographic Testing (RT) Differential absorption of penetrating X-rays or Gamma rays (Iridium-192, Cobalt-60) captured on film or digital flat-panel detector All structural materials Internal volumetric flaws (porosity, slag inclusions, internal cracks parallel to beam) Enclosed hollow engine blades, internal pipe weld roots; severe radiation safety hazards; cannot detect planar cracks perpendicular to beam