Study guide

2.1 Aluminum Alloys, Heat Treatment & Rivet Identification

FAA Aviation Mechanic — Airframe AMA

Track your progress as you read

Finished sections get a check mark.

1 Chapter 1: Introduction & Exam Strategy

1.1 Exam Structure, Eligibility & 14 CFR Part 65 Requirements 1.2 Study Strategy, Blueprint Weighting & Core Formulas

2 Chapter 2: Metallic Structures & Sheet Metal Repair

2.1 Aluminum Alloys, Heat Treatment & Rivet Identification 2.2 Rivet Layout, Edge Distance, Spacing & Driving Standards 2.3 Sheet Metal Layout: Bend Allowance, Setback & Forming 2.4 Sheet Metal Inspection, Damage Evaluation & Flush/Lap Repairs

3 Chapter 3: Non-Metallic Structures: Composites, Wood, Fabric & Transparent Plastics

3.1 Advanced Composites: Fiber Types, Resin Matrices & Core Materials 3.2 Composite Damage Assessment, Repair Methods & Shop Safety 3.3 Aircraft Wood Structures: Defects, Allowable Repairs & Gluing 3.4 Aircraft Fabric Covering, Inspection & Doping/Finishing Processes 3.5 Transparent Plastics, Windows, Windshields & Cabin Interiors

4 Chapter 4: Welding & Structural Fasteners

4.1 Oxyacetylene & Electric Arc Welding Principles for Aviation 4.2 Tubular Steel Fuselage Inspection, Defect Types & Approved Repairs 4.3 Special Structural Fasteners, Blind Rivets & Precision Hardware

5 Chapter 5: Flight Controls, Assembly & Rigging

5.1 Primary and Secondary Flight Control Surfaces & Aerodynamics 5.2 Control Cables, Tensiometers & Temperature-Compensated Rigging 5.3 Turnbuckles, Cable Safetying, Pulleys & Fairleads 5.4 Control Surface Travel, Mass Balancing & Flutter Prevention

6 Chapter 6: Hydraulic & Pneumatic Power Systems

6.1 Hydraulic Fluids, Seal Materials & Contamination Control 6.2 Hydraulic Reservoirs, Power Pumps & Accumulators 6.3 Hydraulic Valves: Pressure, Flow & Directional Control 6.4 High-Pressure Pneumatic Systems, Air Compressors & Moisture Control

7 Chapter 7: Aircraft Landing Gear Systems

7.1 Oleo Shock Struts: Servicing, Air/Oil Charging & Metering Pins 7.2 Retraction Mechanisms, Down-Locks, Alignment & Torque Links 7.3 Aircraft Brakes, Multi-Disc Systems & Anti-Skid Operations 7.4 Aircraft Tires, Wheels, Bearings & Emergency Extension Systems

8 Chapter 8: Aircraft Fuel Systems

8.1 Fuel Tank Types: Rigid, Bladder & Integral (Wet Wing) Tanks 8.2 Fuel System Plumbing: Boost Pumps, Selector Valves & Filtration 8.3 Crossfeed, Fuel Jettison, Fuel Quantity Indication & Probes 8.4 Fuel System Maintenance, Defueling & Tank Confined-Space Safety

9 Chapter 9: Airframe Electrical Systems

9.1 AC & DC Power Generation: Alternators, Inverters & TRUs 9.2 Aircraft Electrical Distribution, Bus Architecture & Circuit Protection 9.3 Aircraft Wire Selection (MIL-W-5086 / MIL-W-22759), Sizing & Bundling 9.4 Bonding, Grounding, Static Dischargers & Electrical Troubleshooting

10 Chapter 10: Cabin Atmosphere & Environmental Control

10.1 Vapor-Cycle & Air-Cycle Machine (ACM) Refrigeration Systems 10.2 Cabin Pressurization: Outflow Valves, Safety Valves & Regulators 10.3 Heating Systems: Combustion Heaters, Exhaust Muffs & Bleed Air 10.4 Aircraft Oxygen Systems: Continuous-Flow, Diluter-Demand & Generators

11 Chapter 11: Aircraft Instrument Systems

11.1 Pitot-Static Systems: Altimeter, VSI, Airspeed & Error Diagnosis 11.2 Gyroscopic Flight Instruments: Rigidity, Precession & Power Sources 11.3 Engine & System Instruments: Bourdon Tubes, Synchros & EICAS 11.4 Instrument Installation, Magnetic Compass Swing & Regulatory Inspections

12 Chapter 12: Communication, Navigation & Warning Systems

12.1 VHF/HF Communications, Antennas & Coaxial Cable Installation 12.2 Navigation Systems: VOR, ILS, DME, ADF, GPS & Weather Radar 12.3 Transponders, Altitude Encoders & Emergency Locator Transmitters 12.4 Position & Warning Systems: Landing Gear Horns, Stall & Warning

13 Chapter 13: Ice, Rain & Fire Protection Systems

13.1 Ice Detection, Pneumatic Deice Boots & Electrothermal Systems 13.2 Wing & Cowl Thermal Bleed-Air Anti-Ice Systems & Rain Removal 13.3 Fire & Smoke Detection: Spot Detectors, Continuous Loops & Optical Sensors 13.4 Fire Extinguishing Systems: HRD Containers, Squibs & Two-Shot Architecture

14 Chapter 14: Airframe Inspection & Maintenance Regulations

14.1 14 CFR Part 43 Appendix D: Scope of 100-Hour & Annual Inspections 14.2 Airworthiness Directives (ADs), Service Bulletins & Major Alterations 14.3 FAA Form 337 Execution, Maintenance Record Entries & Logbook Rules 14.4 Airframe Corrosion Identification, Treatment, Chemical Conversion & NDT

15 Chapter 15: Rotorcraft Fundamentals

15.1 Rotorcraft Aerodynamics, Rotor System Classifications & Flight Controls 15.2 Rotor Blades, Transmissions, Drive Systems & Skid Landing Gear Inspection 15.3 Rotor Track & Balance, Vibration Diagnosis & Helicopter Ground Safety

16 Chapter 16: Water & Waste Systems

16.1 Potable Water Systems: Components, Operation, Servicing & Sanitizing 16.2 Lavatory Waste Systems: Vacuum & Recirculating Types, Servicing & Safety

2.1 Aluminum Alloys, Heat Treatment & Rivet Identification

Key Takeaways Explain This Topic AI

The 4-digit aluminum designation system classifies alloys by primary alloying element: 2xxx (Copper), 3xxx (Manganese), 5xxx (Magnesium), 6xxx (Silicon & Magnesium), and 7xxx (Zinc).

Alclad materials feature a high-strength aluminum alloy core bonded with pure aluminum surface layers (2.5% to 5% thickness per side) providing sacrificial galvanic corrosion protection.

Temper designations indicate thermal and mechanical processing: -O (annealed), -T3 (solution heat-treated and cold-worked), -T4 (naturally aged), and -T6 (artificially precipitation aged).

Solid rivets are identified by distinct head markings: 1100 (A - plain), 2117 (AD - dimple), 2017 (D - raised dot), 2024 (DD - two raised dashes), 5056 (B - raised cross), and 7050 (E - raised circle/triangle).

Icebox rivets (2017-D and 2024-DD) must be refrigerated at or below 32°F (0°C) immediately after quenching to delay precipitation hardening, and driven within 15 to 20 minutes (for 2024-DD) once removed.

Last updated: August 2026

Aluminum Alloys, Heat Treatment & Rivet Identification

FAA Airframe Exam Focus: Mastery of sheet metal airframe maintenance requires deep knowledge of aluminum alloy metallurgy, temper designations, galvanic corrosion protection in clad sheets, and the rigorous identification of solid rivet alloys by head markings and handling rules (especially icebox rivets).

1. The 4-Digit Aluminum Alloy Designation System

Wrought aluminum alloys utilized in modern aircraft fabrication and structural repair are classified according to the four-digit index system established by the Aluminum Association (ANSI H35.1 / Mil-HDBK-5): Alloy Code = [ Major Element Group (1st Digit) ] + [ Alloy Modification (2nd Digit) ] + [ Purity / Specific Alloy (3rd and 4th Digits) ] \text{Alloy Code} = [\text{Major Element Group (1st Digit)}] + [\text{Alloy Modification (2nd Digit)}] + [\text{Purity / Specific Alloy (3rd and 4th Digits)}] Alloy Code = [ Major Element Group (1st Digit) ] + [ Alloy Modification (2nd Digit) ] + [ Purity / Specific Alloy (3rd and 4th Digits) ] 2 0 2 4

  • │ │ └── Specific alloy identification (in 2xxx–8xxx series)
  • │ └──── Modification to original alloy (0 = original, 1-9 = modifications)
  • └────── Major alloying element group (2 = Copper)

Series Major Alloying Element Key Characteristics & Aircraft Applications Heat Treatable?

1xxx Pure Aluminum ( ≥ 99.00 % \ge 99.00\% ≥ 99.00% purity) High electrical/thermal conductivity, superior corrosion resistance, low mechanical strength. Non-structural applications (avionics cooling baffles, oil tanks, decorative fairings). Non-Heat Treatable (Strain hardening only)

2xxx Copper ( C u Cu C u , typically 2.2 % – 4.9 % 2.2\%\text{--}4.9\% 2.2% – 4.9% ) High tensile strength and fatigue resistance; susceptible to intergranular corrosion unless clad or anodized. Primary airframe structural skin, fuselage frames, stringers, wing ribs (e.g., 2024-T3, 2014). Heat Treatable

3xxx Manganese ( M n Mn M n , ≈ 1.2 % \approx 1.2\% ≈ 1.2% ) Moderate strength, high workability, excellent corrosion resistance. Fuel/oil plumbing, fairings, engine cowlings (e.g., 3003-H14). Non-Heat Treatable

4xxx Silicon ( S i Si S i ) Low melting point, high fluidity. Exclusively used as welding rod wire (e.g., 4043) and brazing alloys. Non-Heat Treatable (except when paired with heat-treatable bases)

5xxx Magnesium ( M g Mg M g ) Good tensile strength, excellent weldability, superior corrosion resistance in salt-spray marine environments. Hydraulic lines, fuel tanks, structural rivets for magnesium structures (e.g., 5052-H32, 5056 rivets). Non-Heat Treatable

6xxx Silicon & Magnesium ( M g 2 S i Mg_2Si M g 2 ​ S i ) Medium strength, high ductility, good corrosion resistance, easily extruded and welded. Structural extrusions, landing gear components, floats, seat tracks (e.g., 6061-T6). Heat Treatable

7xxx Zinc ( Z n Zn Z n , with M g Mg M g & C u Cu C u ) Ultra-high tensile and yield strength ( > 70 – 80 ksi >70\text{--}80\text{ ksi} > 70 – 80 ksi ), high hardness, susceptible to stress corrosion cracking unless overaged (-T73). Upper wing skins (compression loads), spar caps, fuselage bulkheads (e.g., 7075-T6, 7050). Heat Treatable

8xxx Other (Lithium, Iron) Aluminum-Lithium (Al-Li) alloys: Low density ( 8 % – 10 % 8\%\text{--}10\% 8% – 10% lighter), high modulus of elasticity. Modern transport airframes (e.g., 8090, 2099). Heat Treatable

2. Clad Aluminum (Alclad) vs. Bare Aluminum

Because high-strength 2xxx and 7xxx copper- and zinc-bearing alloys are susceptible to pitting and intergranular corrosion, manufacturers produce composite sheets known commercially as Alclad (e.g., Alclad 2024-T3 or Alclad 7075-T6). ┌────────────────────────────────────────────────────────┐ ◄── Pure Aluminum Cladding (2.5% - 5.0% thickness)

  • │ Core Alloy: 2024-T3 │ ◄── High-Strength Base Alloy Core (90% - 95% thickness)
  • │ (High Tensile Strength) │
  • └────────────────────────────────────────────────────────┘ ◄── Pure Aluminum Cladding (2.5% - 5.0% thickness)
  • Mechanics of Cladding & Galvanic Sacrificial Protection

Layer Thickness: Pure aluminum ( ≥ 99.3 % \ge 99.3\% ≥ 99.3% pure or corrosion-resistant alloy 7072) is hot-rolled and metallurgically bonded onto both surfaces of the base alloy core. Each cladding layer constitutes 2.5 % 2.5\% 2.5% to 5.0 % 5.0\% 5.0% of the total sheet thickness (totaling 5 % 5\% 5% to 10 % 10\% 10% cladding across both surfaces).

Electrochemical Potential (Galvanic Protection): Pure aluminum possesses a more negative electrode potential (anodic) compared to the copper-rich core alloy (cathodic). If the surface is scratched or exposed to atmospheric moisture/electrolytes, the pure aluminum layer corrodes sacrificially, protecting the underlying core from pitting and intergranular corrosion.

Shop Handling & Maintenance Mandates:

Never use wire brushes, coarse emery cloth, steel wool, or abrasive scraping tools on Alclad sheets.

Scribing on Alclad must be performed strictly with soft lead pencils, felt markers, or layout dye— never with metallic carbide scriber points, which scratch through the clad layer and cause catastrophic stress-corrosion fatigue cracking.

Chemical conversion coatings (MIL-DTL-5541 / Alodine) must be reapplied immediately if the clad layer is burnished or abraded.

3. Heat Treatment Processes & Temper Designations

Heat treatment alters the mechanical properties of aluminum alloys through controlled heating and quenching cycles. Solution Heat Treat (910°F - 930°F)

  • ┌─────────────────┐
  • │ Soaking Furnace │
  • └────────┬────────┘
  • │ Quench in Cold Water (<10 seconds!)
  • ▼
  • ┌─────────────────┐
  • │ Unstable -W │
  • └────────┬────────┘
  • ┌─────────┴─────────┐
  • ▼ ▼
  • Natural Aging Artificial Aging
  • (Room Temp Aging) (Oven Heat ~250°F-375°F)
  • │ │
  • ▼ ▼
  • T3 / -T4 -T6 Temper
  • Primary Heat Treatment Phases

Solution Heat Treatment: The metal is heated in an electric furnace or molten sodium nitrate salt bath to a critical temperature range ( 910 ∘ F 910^\circ\text{F} 91 0 ∘ F to 930 ∘ F 930^\circ\text{F} 93 0 ∘ F for 2024), holding until copper aluminide ( C u A l 2 CuAl_2 C u A l 2 ​ ) dissolves uniformly into solid solution. It is then quenched within 7 to 10 seconds in cold water. Delayed quenching allows C u A l 2 CuAl_2 C u A l 2 ​ to precipitate at grain boundaries, creating extreme vulnerability to intergranular corrosion .

Precipitation Hardening (Aging):

Natural Aging: Occurs spontaneously at room temperature ( 70 ∘ F 70^\circ\text{F} 7 0 ∘ F ) over several days (e.g., 2024 reaches stable -T4 temper in 96 hours).

Artificial Aging: The metal is reheated in a low-temperature curing oven ( 250 ∘ F 250^\circ\text{F} 25 0 ∘ F to 375 ∘ F 375^\circ\text{F} 37 5 ∘ F ) for a specified duration, driving controlled micro-precipitation to produce maximum tensile and yield strength (e.g., -T6 temper).

Annealing: Heating to 750 ∘ F– 800 ∘ F 750^\circ\text{F}\text{--}800^\circ\text{F} 75 0 ∘ F – 80 0 ∘ F followed by slow, controlled furnace cooling ( 50 ∘ F 50^\circ\text{F} 5 0 ∘ F /hr) relieves all internal stresses, yielding the -O temper (fully annealed, lowest tensile strength, maximum formability for extreme bending/drawing).

Standard Temper Suffixes (ASTM / ANSI)

Suffix Temper Description Metallurgical Condition

-F As Fabricated Products shaped by cold/hot working without thermal control.

-O Annealed Fully recrystallized; softest state with maximum ductility.

-H Strain Hardened (Cold Worked) Applied to non-heat-treatable alloys (e.g., -H14: strain-hardened half-hard; -H32: strain-hardened and stabilized).

-W Solution Heat Treated Unstable condition following quench; naturally age-hardening.

-T3 Solution Heat Treated & Cold Worked Quenched, cold-worked (rolled/stretched), naturally aged to stable state (e.g., 2024-T3 skin).

-T4 Solution Heat Treated & Naturally Aged Quenched and aged at ambient temperature to stable equilibrium.

-T6 Solution Heat Treated & Artificially Aged Quenched and oven precipitation-aged for maximum hardness (e.g., 6061-T6, 7075-T6).

-T73 Solution Heat Treated & Overaged Specially overaged to provide maximum resistance to stress corrosion cracking.

4. Solid Rivet Identification & Head Markings

Solid shank rivets remain the primary structural fastener in sheet metal airframes. The rivet alloy is identified by specific raised or recessed physical markings forged into the manufactured head (per MS20470 Universal Head / MS20426 100 ∘ 100^\circ 10 0 ∘ Flush Countersunk Head standards).

Rivet Alloy Letter Code Head Physical Marking Shear Strength Installation & Heat Treatment Rules

1100 A Plain (Smooth, no mark) 10 ksi 10\text{ ksi} 10 ksi ( 10 , 000 psi 10,000\text{ psi} 10 , 000 psi ) Pure aluminum; non-structural. Driven as received.

2117 AD Single Dimple (Recessed Center) 30 ksi 30\text{ ksi} 30 ksi ( 30 , 000 psi 30,000\text{ psi} 30 , 000 psi ) "Field Rivet." General airframe structure. Driven as received without heat treatment. Most common fastener in aviation.

2017 D Single Raised Dot (Teat / Nipple) 35 ksi 35\text{ ksi} 35 ksi ( 35 , 000 psi 35,000\text{ psi} 35 , 000 psi ) "Icebox Rivet." Must be solution heat-treated and refrigerated at < 32 ∘ F <32^\circ\text{F} < 3 2 ∘ F prior to driving.

2024 DD Two Raised Parallel Dashes (Bars) 41 ksi 41\text{ ksi} 41 ksi ( 41 , 000 psi 41,000\text{ psi} 41 , 000 psi ) "Icebox Rivet." High-stress primary joints. Must be solution heat-treated and kept in sub-zero freezer before driving.

5056 B Raised Cross ( + + + ) 28 ksi 28\text{ ksi} 28 ksi ( 28 , 000 psi 28,000\text{ psi} 28 , 000 psi ) Aluminum-Magnesium alloy. Mandatory for riveting magnesium structures to avoid galvanic dissimilar metal reaction.

7050 E Raised Circle, Triangle, or Cross-Ring 43 ksi 43\text{ ksi} 43 ksi ( 43 , 000 psi 43,000\text{ psi} 43 , 000 psi ) High-strength Zn-Mg-Cu alloy. Driven as received without refrigeration; modern replacement for 2024-DD.

Monel M Recessed Dimple w/ Dot or Plain 49 ksi 49\text{ ksi} 49 ksi ( 49 , 000 psi 49,000\text{ psi} 49 , 000 psi ) Nickel-copper alloy; high temperature, firewall, exhaust, and nickel-steel joints. SOLID RIVET HEAD IDENTIFICATION GUIDE:

  • Plain Dimple Raised Dot Two Dashes Raised Cross Raised Circle
  • ┌───┐ ┌───┐ ┌───┐ ┌───┐ ┌───┐ ┌───┐
  • │ │ │ · │ │ • │ │ ═ │ │ ┼ │ │ ○ │
  • └───┘ └───┘ └───┘ └───┘ └───┘ └───┘
  • 1100 (A) 2117 (AD) 2017 (D) 2024 (DD) 5056 (B) 7050 (E)
  • Non-Struct Field Rivet Icebox Rivet Icebox Rivet For Magnesium High Strength
  • 5. Icebox Rivets: Heat Treatment, Sub-Zero Storage & Driving Windows

Alloys 2017 (D) and 2024 (DD) develop exceptional shear strength through copper-phase precipitation hardening. However, in their fully aged room-temperature state, they are too hard and brittle to drive without cracking the shop head (bucktail) and damaging the sheet metal.

The Refrigeration Protocol

Solution Treatment: Rivets are heated to 910 ∘ F– 950 ∘ F 910^\circ\text{F}\text{--}950^\circ\text{F} 91 0 ∘ F – 95 0 ∘ F in an approved furnace or salt bath and instantly quenched in cold water.

Natural Age Hardening Onset: At room temperature ( 70 ∘ F 70^\circ\text{F} 7 0 ∘ F ):

2024-DD begins hardening within 10 to 15 minutes and reaches full hardness in 24 hours.

2017-D begins hardening within 45 to 60 minutes and fully hardens in 4 days.

Sub-Zero Quench Storage: Storing quenched rivets at temperatures below freezing dramatically retards the molecular migration of solute atoms:

32 ∘ F 32^\circ\text{F} 3 2 ∘ F ( 0 ∘ C 0^\circ\text{C} 0 ∘ C ): Retards hardening for up to 24 hours .

0 ∘ F 0^\circ\text{F} 0 ∘ F ( − 18 ∘ C -18^\circ\text{C} − 1 8 ∘ C ) to − 20 ∘ F -20^\circ\text{F} − 2 0 ∘ F : Retards hardening for several weeks or indefinitely .

Shop Driving Time Windows:

Once removed from the freezer/insulated container, 2024-DD rivets must be driven within 15 to 20 minutes .

2017-D rivets must be driven within 1 hour .

If rivets exceed this driving window at room temperature, they must not be driven. Driving hardened rivets results in cracked bucktails, loose joints, and parent sheet distortion. Over-aged rivets must be returned to the heat-treat facility for re-solution treatment (subject to a maximum of 3 to 5 reheat cycles to prevent core alloy diffusion into the surface layer).