Study guide
4.2 Tubular Steel Fuselage Inspection, Defect Types & Approved Repairs
FAA Aviation Mechanic — Airframe AMA
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Introduction & Exam Strategy
1.1 Exam Structure, Eligibility & 14 CFR Part 65 Requirements 1.2 Study Strategy, Blueprint Weighting & Core Formulas
2 Chapter 2: Metallic Structures & Sheet Metal Repair
2.1 Aluminum Alloys, Heat Treatment & Rivet Identification 2.2 Rivet Layout, Edge Distance, Spacing & Driving Standards 2.3 Sheet Metal Layout: Bend Allowance, Setback & Forming 2.4 Sheet Metal Inspection, Damage Evaluation & Flush/Lap Repairs
3 Chapter 3: Non-Metallic Structures: Composites, Wood, Fabric & Transparent Plastics
3.1 Advanced Composites: Fiber Types, Resin Matrices & Core Materials 3.2 Composite Damage Assessment, Repair Methods & Shop Safety 3.3 Aircraft Wood Structures: Defects, Allowable Repairs & Gluing 3.4 Aircraft Fabric Covering, Inspection & Doping/Finishing Processes 3.5 Transparent Plastics, Windows, Windshields & Cabin Interiors
4 Chapter 4: Welding & Structural Fasteners
4.1 Oxyacetylene & Electric Arc Welding Principles for Aviation 4.2 Tubular Steel Fuselage Inspection, Defect Types & Approved Repairs 4.3 Special Structural Fasteners, Blind Rivets & Precision Hardware
5 Chapter 5: Flight Controls, Assembly & Rigging
5.1 Primary and Secondary Flight Control Surfaces & Aerodynamics 5.2 Control Cables, Tensiometers & Temperature-Compensated Rigging 5.3 Turnbuckles, Cable Safetying, Pulleys & Fairleads 5.4 Control Surface Travel, Mass Balancing & Flutter Prevention
6 Chapter 6: Hydraulic & Pneumatic Power Systems
6.1 Hydraulic Fluids, Seal Materials & Contamination Control 6.2 Hydraulic Reservoirs, Power Pumps & Accumulators 6.3 Hydraulic Valves: Pressure, Flow & Directional Control 6.4 High-Pressure Pneumatic Systems, Air Compressors & Moisture Control
7 Chapter 7: Aircraft Landing Gear Systems
7.1 Oleo Shock Struts: Servicing, Air/Oil Charging & Metering Pins 7.2 Retraction Mechanisms, Down-Locks, Alignment & Torque Links 7.3 Aircraft Brakes, Multi-Disc Systems & Anti-Skid Operations 7.4 Aircraft Tires, Wheels, Bearings & Emergency Extension Systems
8 Chapter 8: Aircraft Fuel Systems
8.1 Fuel Tank Types: Rigid, Bladder & Integral (Wet Wing) Tanks 8.2 Fuel System Plumbing: Boost Pumps, Selector Valves & Filtration 8.3 Crossfeed, Fuel Jettison, Fuel Quantity Indication & Probes 8.4 Fuel System Maintenance, Defueling & Tank Confined-Space Safety
9 Chapter 9: Airframe Electrical Systems
9.1 AC & DC Power Generation: Alternators, Inverters & TRUs 9.2 Aircraft Electrical Distribution, Bus Architecture & Circuit Protection 9.3 Aircraft Wire Selection (MIL-W-5086 / MIL-W-22759), Sizing & Bundling 9.4 Bonding, Grounding, Static Dischargers & Electrical Troubleshooting
10 Chapter 10: Cabin Atmosphere & Environmental Control
10.1 Vapor-Cycle & Air-Cycle Machine (ACM) Refrigeration Systems 10.2 Cabin Pressurization: Outflow Valves, Safety Valves & Regulators 10.3 Heating Systems: Combustion Heaters, Exhaust Muffs & Bleed Air 10.4 Aircraft Oxygen Systems: Continuous-Flow, Diluter-Demand & Generators
11 Chapter 11: Aircraft Instrument Systems
11.1 Pitot-Static Systems: Altimeter, VSI, Airspeed & Error Diagnosis 11.2 Gyroscopic Flight Instruments: Rigidity, Precession & Power Sources 11.3 Engine & System Instruments: Bourdon Tubes, Synchros & EICAS 11.4 Instrument Installation, Magnetic Compass Swing & Regulatory Inspections
12 Chapter 12: Communication, Navigation & Warning Systems
12.1 VHF/HF Communications, Antennas & Coaxial Cable Installation 12.2 Navigation Systems: VOR, ILS, DME, ADF, GPS & Weather Radar 12.3 Transponders, Altitude Encoders & Emergency Locator Transmitters 12.4 Position & Warning Systems: Landing Gear Horns, Stall & Warning
13 Chapter 13: Ice, Rain & Fire Protection Systems
13.1 Ice Detection, Pneumatic Deice Boots & Electrothermal Systems 13.2 Wing & Cowl Thermal Bleed-Air Anti-Ice Systems & Rain Removal 13.3 Fire & Smoke Detection: Spot Detectors, Continuous Loops & Optical Sensors 13.4 Fire Extinguishing Systems: HRD Containers, Squibs & Two-Shot Architecture
14 Chapter 14: Airframe Inspection & Maintenance Regulations
14.1 14 CFR Part 43 Appendix D: Scope of 100-Hour & Annual Inspections 14.2 Airworthiness Directives (ADs), Service Bulletins & Major Alterations 14.3 FAA Form 337 Execution, Maintenance Record Entries & Logbook Rules 14.4 Airframe Corrosion Identification, Treatment, Chemical Conversion & NDT
15 Chapter 15: Rotorcraft Fundamentals
15.1 Rotorcraft Aerodynamics, Rotor System Classifications & Flight Controls 15.2 Rotor Blades, Transmissions, Drive Systems & Skid Landing Gear Inspection 15.3 Rotor Track & Balance, Vibration Diagnosis & Helicopter Ground Safety
16 Chapter 16: Water & Waste Systems
16.1 Potable Water Systems: Components, Operation, Servicing & Sanitizing 16.2 Lavatory Waste Systems: Vacuum & Recirculating Types, Servicing & Safety
4.2 Tubular Steel Fuselage Inspection, Defect Types & Approved Repairs
Key Takeaways Explain This Topic AI
A structurally acceptable weld in 4130 steel requires 100% root penetration, a uniform ripple bead with 1/16" to 1/8" reinforcement, feathered edges with base metal, and zero undercutting, overlap, or cracks.
Nondestructive inspection (NDI) of steel tubular airframes relies on visual examination with a 10x optical magnifier and Magnetic Particle Inspection (MPI) to identify surface and subsurface cracks.
AC 43.13-1B authorizes 30° scarf and 90° fishmouth sleeve repairs for 4130 tubing, which increases weld seam length by over 200% and converts direct tensile stress into shear stress.
Rosette welds secure reinforcement sleeves to parent tubes: outer sleeve repairs require rosette holes drilled through the sleeve with a diameter equal to 1/4 the sleeve outside diameter (min 1/4"), filled from the bottom up.
Repairs at tubular cluster nodes and engine mounts are strictly restricted; engine mounts cannot be spliced between nodes without factory alignment jigs and manufacturer-approved engineering data.
Last updated: August 2026
4.2 Tubular Steel Fuselage Inspection, Defect Types & Approved Repairs
FAA Airframe Standard: Steel tubular fuselage structures—common in general aviation, aerobatic aircraft, and agricultural airframes—require meticulous structural inspection and standardized repair procedures. An AMT must be skilled at identifying weld discontinuities, applying Nondestructive Inspection (NDI) techniques, and executing FAA-approved tubular splice repairs under AC 43.13-1B Chapter 4 .
1. Welded Tubular Structure Quality Indicators & Defect Taxonomy
A sound aircraft structural weld must exhibit uniform metallurgical fusion between the filler metal and parent base metal across the entire joint. CROSS-SECTION OF AN ACCEPTABLE AIRCRAFT FILLET / BUTT WELD:
- Weld Reinforcement (1/16" to 1/8" Height)
- ┌─────────┴─────────┐
- │ _ . - . _ │
. - ' ~ ~ ' - .
. ' ' .
- ────────┴─────────────────────────────────────────┴──────── Base Metal
- ████████ ████████ (SAE 4130)
- █████████ █████████
- ███████████_ _███████████
- ────────────▀▀▄▄_ _▄▄▀▀────────────
- ▀▀▄▄_ _▄▄▀▀
- ▀▀▀▀▀▀▀▀▀▀▀▀▀
- └───┬───┘
- 100% Root Penetration
- A. Characteristics of an Acceptable Aviation Weld
Uniform Bead Width: The bead width should be consistent, typically 2 to 3 times the wall thickness 2\text{ to }3\text{ times the wall thickness} 2 to 3 times the wall thickness ( 2 – 3 t 2\text{--}3t 2 – 3 t ) of the base tube.
Reinforcement Height: The crown of the weld should extend 1 / 16 in 1/16\text{ in} 1/16 in to 1 / 8 in 1/8\text{ in} 1/8 in ( 1.6 – 3.2 mm 1.6\text{--}3.2\text{ mm} 1.6 – 3.2 mm ) above the parent metal surface. It must not be flush (underfilled) or excessively crowned (overfilled, causing severe stress concentration).
Root Penetration: The weld must exhibit 100 % 100\% 100% full penetration through the root face, fusing the entire wall thickness without excessive drop-through, icicles, or burn-through inside the tube bore.
Feathered Toe Profile: The edges (toes) of the weld bead must taper smoothly into the base metal with a flat or slightly convex profile, creating a contact angle that minimizes notch effect stress concentrations.
Surface Appearance: Clean, uniform ripple pattern, free from scale, oxide crusts, soot, or heavy slag inclusions.
B. Classification of Structural Weld Defects
Defect Name Physical Description & Manifestation Primary Root Cause Structural Consequence & Repair Action
Undercutting A sharp groove or channel melted into the base metal along the weld toe, left unfilled by filler metal. Excessive welding current/heat, incorrect torch angle, excessive arc length, or travel speed too fast. Critical stress riser. Severely reduces tube fatigue life. Minor undercuts may be blended and re-welded; severe undercuts require tube section replacement.
Cold Lap (Lack of Fusion / Overlap) Weld metal overflows onto the base metal surface without melting into or metallurgically bonding with it. Insufficient heat input, torch angle directed too much on filler rod, dirty/greasy base metal, or slow travel speed. Zero bond strength. Acts as an internal crack initiator. Must be completely ground out to clean sound metal and re-welded.
Porosity (Gas Pockets) Spherical or tubular gas cavities/voids trapped within the solidifying weld metal. Surface contamination (oil, rust, moisture, paint), contaminated filler rod, inadequate shielding gas flow, or wind drafts. Reduces effective cross-sectional shear area. Cluster porosity exceeding 1 / 3 1/3 1/3 wall thickness requires weld cut-out.
Burn-Through Open holes melted through the tube wall, accompanied by large hanging oxide icicles inside the tube. Excessive heat input, travel speed too slow, or excessively large torch tip on thin-wall tubing ( < 0.035 in <0.035\text{ in} < 0.035 in ). Destroys internal tube integrity. Section must be cut out and sleeved per AC 43.13-1B.
Cracks (Hot & Cold) Linear fractures: Hot cracks in weld bead center; Cold cracks in HAZ parallel to toe. High shrinkage stresses, rigid joint clamping, rapid quenching, hydrogen embrittlement, or dirty parent metal. Mandatory rejection. Any crack is grounds for immediate cut-out and structural replacement.
2. Nondestructive Inspection (NDI) Methods for Welded Airframes
Nondestructive inspection methods allow evaluation of structural integrity without damaging the aircraft components. +-----------------------------------------------------------------------------------------+
- | NDI METHODS FOR WELDED AIRCRAFT STRUCTURES |
- +---------------------+-------------------------------+-----------------------------------+
- | Method | Flaw Detection Scope | Material Suitability |
- +---------------------+-------------------------------+-----------------------------------+
- | Visual (VT - 10x) | Surface flaws, bead profile | All materials (First step) |
- | Magnetic Particle | Surface & near-surface cracks | Ferromagnetic only (4130 Steel) |
- | Liquid Penetrant | Surface-breaking cracks/pores | Non-porous (Al, Ti, Stainless) |
- | Radiography (RT) | Internal voids, root fusion | Critical assemblies, engine mounts|
- +---------------------+-------------------------------+-----------------------------------+
- A. Visual Inspection (VT)
Visual inspection using a 10x optical magnifier (loupe) under strong oblique lighting is the mandatory initial inspection technique for all airframe structures. Welded joints must be thoroughly cleaned of paint, scale, and grease using plastic media blasting, chemical strippers, or fine wire brushing prior to inspection.
B. Magnetic Particle Inspection (MPI / MT)
Magnetic Particle Inspection is the standard gold-standard NDI method for ferromagnetic materials (SAE 4130 steel) .
Principle of Operation: An electromagnetic yoke (AC or DC) induces a strong magnetic flux field through the 4130 tube. If a crack or discontinuity exists perpendicular to the flux lines, magnetic flux leaks out into the air, creating localized north and south magnetic poles ( magnetic flux leakage ).
Particle Application: Finely divided ferromagnetic particles (either dry colored powder or wet fluorescent suspension in light petroleum distillate) are applied to the joint. The leaking magnetic poles attract the particles, creating a sharp, highly visible indication of the flaw under white light or UV-A black light (365 nm wavelength) .
Demagnetization Mandate: Following MPI, the component retains residual magnetism that can interfere with aircraft magnetic compasses and attract abrasive iron filings. The part must be thoroughly demagnetized by passing it through a decaying AC demagnetizing coil and verified with a calibrated field indicator (gauss meter, reading < 2 Gauss <2\text{ Gauss} < 2 Gauss ).
3. Approved Tubular Splice Repairs per AC 43.13-1B (Scarf & Fishmouth)
When an aircraft tubular fuselage member is bent, dented, cracked, or corroded, the damaged section must be repaired in strict accordance with FAA Advisory Circular AC 43.13-1B, Chapter 4, Section 5 . WHY SCARF & FISHMOUTH JOINTS ARE MANDATORY OVER 90° BUTT JOINTS:
- 1. REJECTED: 90° Circumferential Butt Joint
- ┌──────────────┬──────────────┐
│ │ │ ◄── 100% of weld seam is in pure direct tension/bending.
└──────────────┴──────────────┘ Smallest weld area (Perimeter = π·D). High stress riser!
- 2. APPROVED: 30° Scarf Joint (AC 43.13-1B)
- ┌─────────────/──────────────┐
- │ / │ ◄── Weld length > 200% of perimeter. Stresses converted
└───────────/────────────────┘ from direct tension into shear loads across joint!
- 3. APPROVED: Fishmouth Joint (30° Angle to Centerline / 60° Included Apex)
- ┌────────────\───────────────┐
- │ > │ ◄── Balances torsional, compressive, and bending loads
└────────────/───────────────┘ symmetrically across tube circumference.
A. The Geometry of Tubular Joints
A standard 90 ∘ 90^\circ 9 0 ∘ perpendicular butt weld around a tube concentrates all bending and tensile stresses across the smallest possible perimeter ( P = π D P = \pi D P = π D ) in direct tension. Under cyclic vibration and aerodynamic gust loads, 90 ∘ 90^\circ 9 0 ∘ butt welds are prone to fatigue failure.
30 ∘ 30^\circ 3 0 ∘ Scarf Cut: The tube is cut at an angle of 30 ∘ 30^\circ 3 0 ∘ relative to the longitudinal tube axis (or 60 ∘ 60^\circ 6 0 ∘ to the perpendicular). This increases the total weld surface area by more than 200 % 200\% 200% , placing the majority of structural loads in shear rather than direct tension.
Fishmouth Cut: The tube sleeve is cut with a 30 ∘ 30^\circ 3 0 ∘ angle from the centerline on both sides, creating a 60 ∘ 60^\circ 6 0 ∘ included apex angle . This distributes torsional and bending loads symmetrically across the entire circumference. +-----------------------------------------------------------------------------------------+
- | AC 43.13-1B APPROVED TUBULAR SPLICE REPAIR METHODS |
- +------------------------------------+----------------------------------------------------+
- | Parameter | Inner Sleeve Repair | Outer Sleeve Repair |
- +------------------------------------+----------------------------+-----------------------+
- | Replacement Tube Material | SAE 4130 (same OD & wall) | SAE 4130 (same OD/t) |
- | Sleeve Outside Diameter | Matches parent inside ID | One gauge size larger |
- | Cut Angle at Splice Joint | 30° Scarf cut | 30° Scarf or Fishmouth|
- | Gap Between Parent Tube Ends | 1/16" to 1/8" (1.6–3.2 mm) | 1/16" to 1/8" |
- | Rosette Welds Required | 4 holes per side (8 total) | 2 to 4 holes per side |
- | Rosette Hole Diameter | 1/4" (or 1/4 parent OD) | 1/4" (or 1/4 sleeve OD|
- | Rosette Hole Spacing | Staggered at 90° intervals | Staggered along sleeve|
- +------------------------------------+----------------------------+-----------------------+
- B. Inner Sleeve Splice Repair (AC 43.13-1B Figure 4-15)
The inner sleeve splice is utilized when external clearance must be maintained (e.g., clearance with fabric covering, control cables, or fairings):
The damaged tube section is cut out cleanly at a 30 ∘ 30^\circ 3 0 ∘ scarf angle .
A replacement tube section of the exact same diameter, material (4130), and wall thickness is prepared with matching 30 ∘ 30^\circ 3 0 ∘ scarf cuts at each end.
An inner sleeve tube is selected with an outside diameter ( O D sleeve OD_{\text{sleeve}} O D sleeve ) that fits snugly inside the parent tube's inside diameter ( I D orig ID_{\text{orig}} I D orig ), with a wall thickness equal to or greater than the original tube.
The inner sleeve must extend at least 1.5 times the parent tube diameter 1.5\text{ times the parent tube diameter} 1.5 times the parent tube diameter on each side of the cut seam.
Rosette Weld Layout: Drill four rosette holes through the parent tube on each side of the joint (total 8 holes). Rosette holes must be 1 / 4 in 1/4\text{ in} 1/4 in diameter (or 1 / 4 of the parent tube OD 1/4\text{ of the parent tube OD} 1/4 of the parent tube OD ) , spaced at least 1 / 2 in 1/2\text{ in} 1/2 in apart, and staggered radially at 90 ∘ 90^\circ 9 0 ∘ intervals around the circumference.
A 1 / 16 in 1/16\text{ in} 1/16 in to 1 / 8 in 1/8\text{ in} 1/8 in gap is left between the parent tube and replacement tube at the scarf seam. This ensures the weld arc penetrates fully and fuses into the underlying inner sleeve. INNER SLEEVE SPLICE REPAIR (AC 43.13-1B FIG 4-15):
- Parent Tube (4130) 1/16"-1/8" Gap Replacement Tube (4130)
- ┌───────────────────────┬─/─┬──────────────────────────────────────────┐
- │ (·) (·) │/ /│ (·) (·) │
- │ / / │ │
- │ (·) (·) / / │ (·) (·) │
- └─────────────────────/─┴─/─┴──────────────────────────────────────────┘
- ▲ ▲ ▲
- │ │ └─── 30° Scarf Cut (Weld penetrates to inner sleeve)
- └──┴──────────────────────── Rosette Welds (1/4" Dia, 4 per side, staggered 90°)
- C. Outer Sleeve Splice Repair (AC 43.13-1B Figure 4-16 & 4-17)
The outer sleeve splice is used when external clearance permits:
The replacement tube is fitted into the cutout gap using square 90 ∘ 90^\circ 9 0 ∘ butt ends or 30 ∘ 30^\circ 3 0 ∘ scarf cuts.
An outer sleeve tube is selected from 4130 stock with an inside diameter that telescopes snugly over the parent tube ( I D sleeve = O D orig ID_{\text{sleeve}} = OD_{\text{orig}} I D sleeve = O D orig ), typically one standard commercial size larger ( 1 / 8 in 1/8\text{ in} 1/8 in larger outside diameter).
The ends of the outer sleeve are cut at a 30 ∘ 30^\circ 3 0 ∘ scarf angle or 60 ∘ 60^\circ 6 0 ∘ fishmouth angle ( 30 ∘ 30^\circ 3 0 ∘ to tube centerline).
The sleeve must overlap the parent tube by at least 1.5 times the sleeve diameter 1.5\text{ times the sleeve diameter} 1.5 times the sleeve diameter beyond the cut joint.
Rosette Welds: Rosette holes are drilled through the outer sleeve only (never through the parent tube). Hole diameter is 1 / 4 in 1/4\text{ in} 1/4 in (or 1 / 4 of sleeve OD 1/4\text{ of sleeve OD} 1/4 of sleeve OD ) , drilled at least 1 / 2 in 1/2\text{ in} 1/2 in from the fishmouth throat.
- 4. Rosette Welds & Internal Corrosion Protection
- A. Rosette Weld Execution Mechanics
A rosette weld is a plug weld designed to lock a reinforcing sleeve mechanically to the underlying parent tube, preventing axial slippage and transferring torsional and shear loads:
Drilling: Holes are drilled and carefully deburred. All metal shavings must be vacuumed out of the joint.
Welding Sequence: The welder strikes the arc at the bottom of the hole onto the inner tube surface , establishing a molten pool and ensuring 100 % 100\% 100% fusion into the inner tube wall before spiraling the arc outward and upward to melt the edges of the outer sleeve hole.
Reinforcement: The hole is filled completely with filler metal, leaving a flat or slightly convex bead. Underfilling creates an unbonded hollow void that fails under shear.
B. Internal Corrosion Ingestion & Sealing
Unlike sheet metal wings, the inside surfaces of closed steel tubular fuselages cannot be inspected visually after fabrication:
Hot Linseed Oil / Paralketone Treatment: After all welding repairs on a closed tubular bay are completed and cooled, the interior of the tubing must be protected. Hot boiled linseed oil (heated to 160 ∘ F– 180 ∘ F 160^\circ\text{F}\text{--}180^\circ\text{F} 16 0 ∘ F – 18 0 ∘ F / 71 ∘ C– 82 ∘ C 71^\circ\text{C}\text{--}82^\circ\text{C} 7 1 ∘ C – 8 2 ∘ C ) or a rust-inhibiting compound (MIL-PRF-16173) is pumped under pressure into the lowest point of the bay through a small drilled hole ( 1 / 16 in 1/16\text{ in} 1/16 in to 1 / 8 in 1/8\text{ in} 1/8 in ).
The oil is allowed to fill the entire bay and coat all internal surfaces. The oil is then completely drained out, leaving a sealed corrosion-resistant film.
Plugging: The drain and vent holes are permanently sealed by installing blind rivets, cadmium-plated drive screws, or seal welds to prevent moisture and oxygen ingress.
5. Cluster Bay Repairs & Engine Mount Limitations CLUSTER JOINT REPAIR RESTRICTIONS:
- Gusset Plate (4130 Sheet, 1.0x to 1.25x t)
- ┌─────────────────┐
- │ ▲ │
- │ / \ │
- Tube A ─────┼──────/ \──────┼───── Tube B
- │ / * \ │
- │ /_______\ │
- └────────┬────────┘
- │
- Tube C
* CRITICAL MANDATE: Splice cuts must NEVER terminate at the cluster node weld!
Splice sleeves must be offset into the open bay at least 1.5D away from node.
A. Cluster Joint & Bay Repairs
A cluster joint is a structural intersection where three or more fuselage tubing members converge at a single node:
Never Cut at the Node: Repair splices must never terminate directly at the welded cluster node . Splicing directly onto a multi-tube intersection creates extreme thermal stress concentration and destroys adjacent tube temper.
Offsetting the Splice: The damaged tube must be cut off at least 1.5 to 2.0 tube diameters 1.5\text{ to }2.0\text{ tube diameters} 1.5 to 2.0 tube diameters away from the cluster intersection , allowing an outer or inner sleeve splice to be executed in the straight bay section.
Gusset Reinforcement: Cracked or distorted cluster joints may be structurally reinforced by welding form-fitted gusset plates ( 4130 4130 4130 sheet metal, thickness equal to 1.0 to 1.25 times 1.0\text{ to }1.25\text{ times} 1.0 to 1.25 times the thickest tube wall ) across the acute angles of the intersection.
B. Engine Mount Repair Limitations
Aircraft engine mounts are dynamic, highly stressed structures subjected to combined multi-axis loads: engine weight (cantilever bending), propeller thrust (tension/compression), gyroscopic precession (torsion), and severe reciprocating/turbine vibration.
Important
FAA Major Repair Limitation: Splicing or sectioning damaged engine mount tubing is strictly restricted . Most airframe manufacturers prohibit field-splicing engine mount members. An engine mount can only be repaired if explicit repair drawings exist in the Manufacturer's Structural Repair Manual (SRM). Furthermore, all repairs must be performed in an approved factory alignment jig to prevent even microscopic misalignment of the engine thrust line. Without an approved jig and data, a damaged engine mount must be replaced.