Study guide
4.6 Soldering, Welding & Weld Quality Inspection
FAA Aviation Mechanic — General AMG
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Introduction & AMG Exam Overview
1.1 About the FAA Aviation Mechanic General Knowledge Test 1.2 How to Study for the AMG Exam
2 Chapter 2: Maintenance Forms, Records, Publications & Regulations
2.1 14 CFR Parts 43, 65, and 91 Regulatory Framework 2.2 Aviation Mechanic Privileges, Limitations & Recent Experience 2.3 Maintenance Recordkeeping & Return-to-Service Entries (14 CFR 43.9 & 43.11) 2.4 FAA Form 337 Major Repairs and Major Alterations 2.5 Airworthiness Directives (ADs) & Mandatory Compliance 2.6 Type Certificate Data Sheets (TCDS), STCs, ACs & Maintenance Manuals 2.7 FAA Forms, MMEL/MEL, Inoperative Equipment & Parts Effectivity
3 Chapter 3: Basic Electricity
3.1 DC Electrical Circuits, Ohm's Law & Power 3.2 AC Electrical Fundamentals, Reactance & Impedance 3.3 Aircraft Lead-Acid & Nickel-Cadmium Storage Batteries 3.4 DC Generators, Alternators & Electric Motors 3.5 Aircraft Wiring, Bonding & Circuit Protection Devices 3.6 Resistor Color Codes, Semiconductors, Digital Logic & Electrostatic Discharge
4 Chapter 4: Materials & Processes
4.1 Aircraft Ferrous and Nonferrous Metals & Heat Treatment 4.2 Metal Hardness Testing (Rockwell, Brinell, Vickers) 4.3 Nondestructive Testing (NDT/NDI) Inspection Methods 4.4 Aircraft Hardware, Fasteners & Safetying Methods 4.5 Composite Materials, Plastics & Control Cables 4.6 Soldering, Welding & Weld Quality Inspection
5 Chapter 5: Cleaning & Corrosion Control
5.1 Corrosion Types, Chemistry & Identification 5.2 Corrosion Removal, Chemical Conversion Coatings & Surface Treatments 5.3 Aircraft Cleaning Agents, Precautions & Preventative Maintenance 5.4 Aircraft Finishing Systems, Registration Markings & Placards
6 Chapter 6: Weight & Balance
6.1 Weight and Balance Terminology, Datum, Arm & Moment Principles 6.2 Aircraft Weighing Procedures, Scale Reactions & Tare Weight 6.3 Center of Gravity Computations, Extreme Loading & Ballast
7 Chapter 7: Ground Operation, Servicing & Safety
7.1 Engine Starting Procedures, Danger Areas & Ground Taxi Safety 7.2 Aircraft Servicing (Oxygen, Hydraulic, Pneumatic & De-Icing Fluids) 7.3 Aircraft Fueling Safety, Static Grounding & Hangar Fire Protection 7.4 Airport Movement Areas, Hazardous Materials, Tool Control & FOD Prevention
8 Chapter 8: Aircraft Drawings
8.1 Aircraft Drawing Types, Title Blocks & Orthographic Projections 8.2 Line Conventions, Dimensions, Tolerances & Material Symbols 8.3 Electrical Wiring Diagrams, Logic Flowcharts & Fluid Schematics
9 Chapter 9: Fluid Lines & Fittings
9.1 Rigid Metal Tubing Fabrication, Bending & 37° AN Flaring 9.2 Flexible Hose Construction, Pressure Ratings & Lay Lines 9.3 AN/MS/Quick-Disconnect Fittings, Identification & Installation
10 Chapter 10: Mathematics for Aviation Maintenance
10.1 Fractions, Decimals, Percentages & Ratio/Proportion 10.2 Geometric Computations (Area, Volume & Cylinder Displacement) 10.3 Algebraic Equations, Powers, Roots & Maintenance Conversions
11 Chapter 11: Physics for Aviation Maintenance
11.1 Matter, Mass, Weight, Density & Specific Gravity 11.2 Work, Energy, Power & Simple Machines (Mechanical Advantage) 11.3 Fluid Mechanics, Pascal's Law & Bernoulli's Principle 11.4 Thermodynamics, Heat Transfer, Gas Laws, Sound & Aerodynamics 11.5 Standard Atmosphere, Density & Pressure Altitude, Flight Controls & Aerodynamic Devices
12 Chapter 12: Inspection Concepts, Techniques & Precision Measurement
12.1 Aircraft Inspection Programs & Inspection Concepts 12.2 Precision Measuring Tools & Tool Calibration
13 Chapter 13: Human Factors in Aviation Maintenance
13.1 Human Error, the Dirty Dozen & Maintenance Safety Culture 13.2 Human Performance, Limitations, Fatigue & the Work Environment 13.3 Communication, Shift Turnover, Event Investigation & Professionalism
4.6 Soldering, Welding & Weld Quality Inspection
Key Takeaways Explain This Topic AI
Only non-corrosive rosin flux may be used on aircraft electrical and electronic soldered connections; corrosive acid flux keeps attacking the joint after soldering and is limited to sheet-metal work.
63/37 tin-lead solder is eutectic and freezes at a single temperature with no pasty range, which is why it is preferred for electronics where a disturbed joint would otherwise go cold.
An acceptable weld shows uniform bead width and evenly spaced ripples, uniform height, a smooth taper into the base metal, complete root penetration, no undercut or burn-through, and no cracks.
A defective weld must never be repaired by welding over it: the entire original weld must be ground or machined away to clean parent metal before re-welding, stress relieving, and re-inspecting.
A neutral oxyacetylene flame is used for steel including 4130; an oxidizing flame burns out alloying elements and leaves a brittle weld, while a carburizing flame adds carbon.
Last updated: August 2026
4.6 Soldering, Welding & Weld Quality Inspection
Four knowledge elements of ACS Subject AM.I.E deal with joining metal by melting it: soldering preparation, types of solder, and flux usage ( AM.I.E.K7 ); characteristics of acceptable welds ( K12 ); characteristics of unacceptable welds ( K13 ); and procedures for weld repairs ( K14 ). Skill element AM.I.E.S3 requires you to inspect and check welds during the practical test. This section covers all of them.
1. Soldering: Metallurgy, Flux, and the Cardinal Rules
Soldering joins metals with a filler alloy that melts below the melting point of the base metals, which are not melted at all. The bond is a thin intermetallic layer plus mechanical adhesion — it is not a fusion weld, and it carries a fraction of the strength.
Soft solder alloys
- Alloy (Sn/Pb) Melting behaviour Typical aviation use
- 60/40 tin-lead Melts about 361 °F, pasty range up to about 374 °F General electrical and electronic work
63/37 tin-lead Eutectic — melts and freezes at a single temperature, about 361 °F, with no pasty range Preferred for electronics because there is no plastic phase in which a disturbed joint goes cold
50/50 tin-lead Wider pasty range Sheet-metal and non-electrical tinning work
95/5 tin-antimony and lead-free alloys Higher melting point Higher-temperature and lead-restricted applications
Flux: the rule that gets people violated
Flux chemically removes surface oxide so molten solder can wet the base metal. The choice of flux is a safety decision, not a preference.
Rosin flux (non-corrosive) is the ONLY flux permitted on electrical and electronic connections. Its residue is inert at room temperature.
Acid flux (chloride-based, corrosive) must NEVER be used on electrical work. Its residue keeps attacking the joint and the surrounding wire strands long after the iron is put away, producing a green corroded connection and eventual open circuit. Acid flux is confined to sheet-metal and plumbing work where the residue can be fully washed away.
Always clean the joint — mechanically abrade or chemically clean to bright metal — before fluxing.
Producing an acceptable joint
Make the mechanical connection first. Solder is not a mechanical fastener; a soldered joint must not rely on the solder to hold the parts in position.
Heat the work, not the solder. Apply the iron tip to the joint, then feed solder to the joint , letting the heated metal melt it. Solder melted on the iron and dripped onto a cold joint produces a cold joint every time.
Do not disturb the joint while it freezes.
Judge the result visually. An acceptable joint is bright, smooth, and shiny , with a thin concave fillet through which the outline of the underlying wire is still visible. A cold joint is dull, grainy, or frosted and often bulbous — it must be reheated or remade. An excess-solder joint is a shiny blob that hides the wire outline; it can conceal a poor connection.
Never solder a connection that carries primary structural load, and never solder a control cable terminal — swaged or wrapped-and-soldered cable terminals are governed by the specific approved procedure in AC 43.13-1B and the manufacturer's data.
2. Welding Processes Used on Aircraft
Welding fuses the base metals together, with or without filler, producing a joint as strong as the parent material when it is done correctly.
Process Common name Where you see it on aircraft
Oxyacetylene gas welding Gas welding, torch welding Classic 4130 chrome-molybdenum steel tube fuselages, engine mounts, older exhaust systems
Gas tungsten arc welding (GTAW) TIG, Heliarc The modern standard for 4130 steel, stainless, aluminum, magnesium, and titanium; a non-consumable tungsten electrode with an inert shielding gas
- Gas metal arc welding (GMAW) MIG Production sheet fabrication; less common in field repair
- Shielded metal arc welding (SMAW) Stick Heavy non-aircraft shop work such as tooling and stands
Flame settings for gas welding are an exam item. Adjusting the mixture at the torch produces three distinct flames:
Neutral flame — balanced oxygen and acetylene, a clearly defined rounded white inner cone. This is the general-purpose flame for steel , including 4130.
Carburizing (reducing) flame — excess acetylene, showing a feathery secondary cone around the inner cone. Used for high-carbon steel, nickel, and hard-surfacing; it adds carbon to the puddle.
Oxidizing flame — excess oxygen, a short, sharp, noisy inner cone. Used for brass and bronze; on steel it burns out alloying elements and makes the weld brittle.
Shielding gases. GTAW and GMAW use argon , helium , or argon-helium mixtures to blanket the molten puddle and exclude atmospheric oxygen and nitrogen. Loss of shielding gas produces a grey, sooty, porous bead.
3. Characteristics of an Acceptable Weld (AM.I.E.K12)
FAA AC 43.13-1B gives an inspectable list. A good weld shows all of these:
The bead is of uniform width , and the ripples are evenly spaced along its length.
The bead height is uniform , with the crown neither excessively high nor sunken below the base metal.
The face is smooth , free of gas pockets, pits, and inclusions.
No oxide forms on the base metal more than about one-half inch from the weld.
The weld tapers off smoothly into the base metal — no sudden change in section.
No burned-through areas, and no undercut at the toes.
Complete penetration at the root, with the base metals visibly fused into one another rather than merely coated.
No cracks of any kind, in the weld or in the heat-affected zone.
4. Characteristics of an Unacceptable Weld (AM.I.E.K13)
Defect What you see Usual cause
Undercut A groove melted into the base metal at the toe of the bead, reducing section thickness Excessive current or heat, incorrect torch/electrode angle
Overlap (cold lap) Weld metal rolled over the base metal without fusing to it Insufficient heat, travel too slow
Lack of penetration Root of the joint not fused; a visible unfused line at the back Insufficient heat, travel too fast, poor joint preparation
- Porosity Rounded gas pockets in or on the bead Contamination, loss of shielding gas, moisture, oxidizing flame
- Inclusion Trapped slag, tungsten, or oxide inside the bead Dirty base metal, tungsten touching the puddle
Cracks Any linear separation, hot or cold, in the weld or heat-affected zone Restraint, rapid cooling, wrong filler, hydrogen
Excessive spatter and rough, irregular ripples Uneven, lumpy appearance Wrong current, wrong flame, unsteady travel
- Burn-through A hole melted through thin section Excessive heat on thin wall
- 5. Weld Repair Procedures (AM.I.E.K14)
The single rule most often missed on the test: a defective weld must not be repaired by simply welding over it. Re-melting an existing bead traps the original defect, adds heat cycles, and grows the heat-affected zone.
The correct sequence is:
Completely remove the original weld metal by grinding, filing, or machining down to clean parent metal.
Remove all traces of the defect — a crack must be chased to its ends and eliminated, not blended over.
Prepare the joint (bevel, fit-up, cleanliness) exactly as if it were an original weld.
Re-weld using approved data, appropriate filler, and appropriate process.
Stress-relieve as required by the applicable data. Welded 4130 steel tube structure is normally stress-relieved after welding to relieve residual stresses in the heat-affected zone.
Re-inspect — visually first, then by dye penetrant, magnetic particle, or radiography as the approved data requires.
Two structural limits worth memorizing: repairs to a cluster joint or a splice in a longeron are structural repairs governed by the manufacturer's structural repair manual or AC 43.13-1B, and a welded joint that has been repaired more than the number of times allowed by the applicable data must be replaced, not welded again. Finally, welding on any part that has been heat treated to a specific temper destroys that temper in the heat-affected zone — the part must be re-heat-treated or scrapped per the approved data.