Study guide
11.2 Corrosion Recognition, Control & Damage Limits
FAA Inspection Authorization IAR
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: 14 CFR Part 65 Subpart D — Inspection Authorization
1.1 IA Eligibility, Experience & Application Requirements 1.2 IA Privileges, Limitations & Operational Authority 1.3 Duration, Validity & Biennial Renewal Requirements
2 Chapter 2: 14 CFR Part 43 — Maintenance, Alterations & Performance Standards
2.1 Scope of Part 43 & Authorized Maintenance Personnel 2.2 Major vs. Minor Repairs, Alterations & Preventive Maintenance 2.3 Performance Rules & Standards of Workmanship (14 CFR 43.13)
3 Chapter 3: Determining Airworthiness & Inspection Procedures
3.1 The Two-Part Airworthiness Standard & IA Determination 3.2 Conducting Annual & 100-Hour Inspections (14 CFR 43.15 & Appendix D) 3.3 Progressive Inspections & Disapproval Procedures (14 CFR 43.11 & 91.409)
4 Chapter 4: Airworthiness Directives, Service Bulletins, TCDS & STCs
4.1 Airworthiness Directives: Authority, Applicability & Compliance Tracking 4.2 Type Certificate Data Sheets & Aircraft Specifications 4.3 Manufacturer Service Information & Supplemental Type Certificates
5 Chapter 5: Major Repairs, Alterations, FAA Form 337 & Form 8130-3
5.1 Approved Data vs. Acceptable Data: Legal Standards & Sources 5.2 FAA Form 337: Preparation, Execution & Distribution 5.3 FAA Field Approvals, DER Data & Form 8130-3 Traceability
6 Chapter 6: Weight and Balance Calculations & Adverse Loading Checks
6.1 Weight & Balance Fundamentals, Scale Weighing & EWCG 6.2 Forward and Aft Adverse-Condition Loading Checks 6.3 Ballast Calculations, Equipment Changes & Percent MAC
7 Chapter 7: Technical Publications, Data Precedence & Inoperative Equipment
7.1 Publication Hierarchy, Technical Data Precedence & ICAs 7.2 MMEL vs. Operator MEL: Relief, Operations & Deferral Procedures 7.3 Operating with Inoperative Equipment Without an MEL (14 CFR 91.213(d))
8 Chapter 8: Maintenance Records, Retention, Transfer & Return to Service
8.1 Maintenance Record Entries & Return-to-Service Standards (14 CFR 43.5, 43.7, 43.9) 8.2 Inspection Record Entries & Certification Statements (14 CFR 43.11) 8.3 Record Retention, Aircraft Transfer & Rebuilt Engine Records (14 CFR 91.417, 91.419, 91.421)
9 Chapter 9: Structural Repairs, Sheet Metal Layout & Welded Steel Structure (AC 43.13-1B)
9.1 Sheet Metal Layout: Bend Radius, Setback, Bend Allowance & Sight Lines 9.2 Riveted Repair Design: Rivet Alloys, Substitution, Edge Distance & Spacing 9.3 Welded Steel Tubular Structure: Splices, Sleeves & Engine Mount Repairs
10 Chapter 10: Aircraft Hardware, Control Cables, Fluid Lines & Electrical Standards
10.1 Aircraft Hardware, Control Cables, Turnbuckles & Safetying Methods 10.2 Fluid Lines, Flexible Hose & Minimum Bend Radius Standards 10.3 Electrical Wire Sizing, Conductor Temperature & Load Analysis
11 Chapter 11: Alteration Design Substantiation, Corrosion Control & Powerplant Standards
11.1 Alteration Design Fundamentals: Limit vs. Ultimate Loads & Static Proof Testing 11.2 Corrosion Recognition, Control & Damage Limits 11.3 Powerplant, Propeller & Nondestructive Inspection Standards for the IA
12 Chapter 12: Part 21 Product Certification, Parts Eligibility & Reading Type Data
12.1 Part 21 Certification Framework: TC, PC, PMA, TSO & Owner-Produced Parts 12.2 Reading Type Data: Serial-Number-Specific Lookups & Interpreting Notes 12.3 Airworthiness Certificates, Required Documents, Marking & Registration
11.2 Corrosion Recognition, Control & Damage Limits
Key Takeaways Explain This Topic AI
AC 43.13-1B Chapter 6 covers corrosion inspection and protection, and the FAA AC 43-4 series is the dedicated corrosion control guidance for aircraft.
Dissimilar metal or galvanic corrosion occurs when metals far apart in the galvanic series contact each other in the presence of an electrolyte, and it is prevented by isolating the surfaces.
Intergranular and exfoliation corrosion attack the grain boundaries of aluminum alloys and are far more structurally serious than surface corrosion because material loss extends into the section.
Stress corrosion cracking develops where a sustained tensile stress and a corrosive environment act together, and it produces cracks without visible general corrosion.
Corrosion removal is limited by the allowable damage limits in the manufacturer's structural repair manual; removal beyond those limits converts the situation into a repair requiring approved data.
Last updated: September 2026
11.2 Corrosion Recognition, Control & Damage Limits
Warning
Corrosion is the discrepancy an IA is most likely to under-call. A patch of surface oxide on a stringer looks like housekeeping. Intergranular corrosion in the same location, which can look nearly identical from outside, has removed load-carrying material through the section. The inspection skill is not spotting discoloration — it is classifying what kind of attack produced it, and knowing when the answer stops being "clean and treat" and becomes "this is a major repair."
The guidance is AC 43.13-1B, Chapter 6, Corrosion, Inspection and Protection , supported by the FAA's dedicated corrosion control advisory circular series, AC 43-4 .
Why Corrosion Happens
Corrosion is an electrochemical process requiring four things: an anode , a cathode , a conductive electrolyte path , and an electrical connection between anode and cathode. Break any one and corrosion stops. Every preventive measure in aviation maintenance is an attack on one of those four:
- Preventive Measure Which Element It Breaks
- Paint, primer, sealant, conversion coating Removes the electrolyte path
- Drain holes, ventilation, keeping the aircraft dry Removes the electrolyte
- Isolating dissimilar metals with sealant, tape, or a washer Breaks the electrical connection
- Corrosion-inhibiting compounds in lap joints and cavities Displaces electrolyte and inhibits the reaction
- Alclad cladding on aluminum sheet Sacrificial anode protects the core alloy
Environmental drivers : salt air, industrial atmospheres, high humidity, and standing water. Design drivers : faying surfaces, lap joints, dissimilar metal contact, crevices, and any location where water collects and cannot drain.
- The Types an IA Must Distinguish
- Surface (Uniform Etch) Corrosion
General roughening and dulling of the surface, with a powdery white oxide on aluminum or red rust on steel. It is the least serious form provided it has not progressed inward . Removed mechanically, treated, and refinished.
Pitting
Localized attack producing small, sharp-bottomed holes, most common on aluminum and stainless steel. Pitting is more serious than its appearance suggests because each pit is a stress riser and because depth is hard to judge from the surface. Depth must be measured after cleanout and compared against allowable limits.
Galvanic (Dissimilar Metal) Corrosion
Occurs where two metals far apart in the galvanic series are in contact in the presence of an electrolyte. The less noble (more anodic) metal corrodes preferentially. Classic aircraft cases:
A steel fastener in an aluminum structure — the aluminum corrodes around the fastener.
Magnesium components in contact with aluminum or steel — magnesium is highly anodic and corrodes aggressively, which is why 5056 rivets (magnesium-compatible) are specified in magnesium structure.
Carbon fiber against aluminum — carbon is strongly cathodic and drives severe aluminum corrosion.
Prevention is isolation : sealant, a barrier tape, a compatible primer, or an appropriate washer between the surfaces.
Intergranular Corrosion
Attack along the grain boundaries of an alloy, typically the result of improper heat treatment leaving a difference in electrical potential between grain boundary material and the grain center. It proceeds inside the material and can be extensive while the surface still looks acceptable.
Exfoliation
An advanced form of intergranular corrosion in wrought, extruded, or rolled products, where the corrosion products between grain layers force the layers apart. Recognized by lifting, flaking, or leafing of the surface — the metal delaminates like the pages of a book. Exfoliation on an extruded spar cap or stringer is a serious structural finding, because the section has lost material through its depth.
Filiform
Thread-like worm tracks under paint, usually where a coating was applied over a poorly prepared or contaminated surface, and driven by high humidity. Cosmetic at first, but it undermines the coating and opens the way for other forms.
Fretting
Occurs at faying surfaces subject to slight relative motion under load, producing a black or dark powder and eventually pitting and cracking. Found at bolted joints that have loosened and at bearing interfaces.
Stress Corrosion Cracking
Cracking produced by the combination of a sustained tensile stress and a corrosive environment , often with no general corrosion visible at all. Susceptible locations are those with residual assembly stress — interference-fit bushings, tapered pins, over-torqued clamps, and press-fit fittings. Because it produces cracks rather than material loss, it is found by crack detection methods rather than by looking for oxide.
Quick Recognition Table
- Type Visual Signature Typical Location Structural Seriousness
- Surface Dulling, white powder on aluminum Exposed skins, unprotected surfaces Low if shallow
- Pitting Small sharp-edged holes Aluminum and stainless surfaces Moderate; depth governs
Galvanic Attack concentrated at a metal-to-metal interface Steel fasteners in aluminum, magnesium at any joint Moderate to high
- Intergranular Little surface evidence; internal loss Heat-treated aluminum sections High
- Exfoliation Lifting, leafing, layered flaking Extrusions, spar caps, stringers High
- Filiform Worm tracks under the finish Painted surfaces in humid service Low initially
- Fretting Black powder at a joint Bolted joints with relative motion Moderate to high
- Stress corrosion Cracks with no general corrosion Interference fits, over-torqued clamps High
- Where an IA Looks [ ] Battery box and the structure downstream of the vent
- [ ] Lavatory and galley areas; anywhere fluids are spilled
- [ ] Wheel wells, landing gear bays, and the structure behind gear doors
- [ ] Lower fuselage skins, belly, and bilge; steel tube lower longerons
- [ ] Exhaust trail areas and the structure aft of exhaust outlets
- [ ] Wing and empennage attach fittings; hinges and hinge pins
- [ ] Faying surfaces, lap joints, and under doublers
- [ ] Piano hinges, control surface interiors, and balance weight attachments
- [ ] Float and amphibian structure; any seaplane operated in salt water
- [ ] Under the floorboards and beneath insulation blankets
- [ ] Drain holes: blocked drains are the leading cause of everything above
- Treatment and the Limits That Govern It
The standard sequence is: clean the area, remove the corrosion products, neutralize any remaining residue, restore the protective finish, and record what was done. For aluminum, removal is by mechanical means appropriate to the alloy, followed by a chemical conversion coating and then primer and topcoat. For steel, removal is followed by an appropriate corrosion-preventive finish.
The decisive question is depth, not area. Every airframe manufacturer publishes allowable damage limits — the maximum material thickness that may be removed from a given part before the part is no longer serviceable. So:
Clean out the corrosion completely. Blending around it and painting over the remainder guarantees it returns and hides the extent.
Measure the remaining thickness and compare it with the allowable damage limits in the manufacturer's structural repair manual or maintenance manual.
If removal stayed within the allowable limits , restore the finish, record the work under § 43.9, and note the location so that the next inspection can compare.
If removal exceeded the allowable limits , the part is no longer to type design. It must be repaired using approved data or replaced , and a structural repair to a primary member is a major repair requiring Form 337 (Chapter 5).
There is no fourth option. Cleaning out corrosion past the allowable limits and refinishing without a repair leaves an aircraft that is not airworthy, however clean it looks.
Recording Corrosion Findings
An IA's records serve the next inspector. A useful entry states where (station and structure), what type , how deep after cleanout , what limit it was compared against , and what was done . "Cleaned and treated corrosion, belly" tells the next IA nothing; "Removed light pitting corrosion, right side fuselage skin between stations 120 and 132, maximum depth after cleanout 0.004 inch against allowable 0.008 inch per SRM 53-30-01 Rev 12; conversion coated, primed, topcoated" lets the next inspector detect progression.
High-Yield Exam Traps
Galvanic corrosion attacks the less noble metal. In a steel-fastener-in-aluminum joint, the aluminum goes.
Exfoliation is intergranular corrosion in wrought or extruded product — the leafing appearance is the giveaway, and it is a serious structural finding.
Stress corrosion cracking needs sustained tensile stress plus a corrosive environment , and it can occur with no general corrosion visible.
Depth against allowable damage limits decides the disposition , not the surface area.
Exceeding allowable limits makes it a repair , and on a primary member that means approved data and a Form 337.