Study guide
9.3 Welded Steel Tubular Structure: Splices, Sleeves & Engine Mount Repairs
FAA Inspection Authorization IAR
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: 14 CFR Part 65 Subpart D — Inspection Authorization
1.1 IA Eligibility, Experience & Application Requirements 1.2 IA Privileges, Limitations & Operational Authority 1.3 Duration, Validity & Biennial Renewal Requirements
2 Chapter 2: 14 CFR Part 43 — Maintenance, Alterations & Performance Standards
2.1 Scope of Part 43 & Authorized Maintenance Personnel 2.2 Major vs. Minor Repairs, Alterations & Preventive Maintenance 2.3 Performance Rules & Standards of Workmanship (14 CFR 43.13)
3 Chapter 3: Determining Airworthiness & Inspection Procedures
3.1 The Two-Part Airworthiness Standard & IA Determination 3.2 Conducting Annual & 100-Hour Inspections (14 CFR 43.15 & Appendix D) 3.3 Progressive Inspections & Disapproval Procedures (14 CFR 43.11 & 91.409)
4 Chapter 4: Airworthiness Directives, Service Bulletins, TCDS & STCs
4.1 Airworthiness Directives: Authority, Applicability & Compliance Tracking 4.2 Type Certificate Data Sheets & Aircraft Specifications 4.3 Manufacturer Service Information & Supplemental Type Certificates
5 Chapter 5: Major Repairs, Alterations, FAA Form 337 & Form 8130-3
5.1 Approved Data vs. Acceptable Data: Legal Standards & Sources 5.2 FAA Form 337: Preparation, Execution & Distribution 5.3 FAA Field Approvals, DER Data & Form 8130-3 Traceability
6 Chapter 6: Weight and Balance Calculations & Adverse Loading Checks
6.1 Weight & Balance Fundamentals, Scale Weighing & EWCG 6.2 Forward and Aft Adverse-Condition Loading Checks 6.3 Ballast Calculations, Equipment Changes & Percent MAC
7 Chapter 7: Technical Publications, Data Precedence & Inoperative Equipment
7.1 Publication Hierarchy, Technical Data Precedence & ICAs 7.2 MMEL vs. Operator MEL: Relief, Operations & Deferral Procedures 7.3 Operating with Inoperative Equipment Without an MEL (14 CFR 91.213(d))
8 Chapter 8: Maintenance Records, Retention, Transfer & Return to Service
8.1 Maintenance Record Entries & Return-to-Service Standards (14 CFR 43.5, 43.7, 43.9) 8.2 Inspection Record Entries & Certification Statements (14 CFR 43.11) 8.3 Record Retention, Aircraft Transfer & Rebuilt Engine Records (14 CFR 91.417, 91.419, 91.421)
9 Chapter 9: Structural Repairs, Sheet Metal Layout & Welded Steel Structure (AC 43.13-1B)
9.1 Sheet Metal Layout: Bend Radius, Setback, Bend Allowance & Sight Lines 9.2 Riveted Repair Design: Rivet Alloys, Substitution, Edge Distance & Spacing 9.3 Welded Steel Tubular Structure: Splices, Sleeves & Engine Mount Repairs
10 Chapter 10: Aircraft Hardware, Control Cables, Fluid Lines & Electrical Standards
10.1 Aircraft Hardware, Control Cables, Turnbuckles & Safetying Methods 10.2 Fluid Lines, Flexible Hose & Minimum Bend Radius Standards 10.3 Electrical Wire Sizing, Conductor Temperature & Load Analysis
11 Chapter 11: Alteration Design Substantiation, Corrosion Control & Powerplant Standards
11.1 Alteration Design Fundamentals: Limit vs. Ultimate Loads & Static Proof Testing 11.2 Corrosion Recognition, Control & Damage Limits 11.3 Powerplant, Propeller & Nondestructive Inspection Standards for the IA
12 Chapter 12: Part 21 Product Certification, Parts Eligibility & Reading Type Data
12.1 Part 21 Certification Framework: TC, PC, PMA, TSO & Owner-Produced Parts 12.2 Reading Type Data: Serial-Number-Specific Lookups & Interpreting Notes 12.3 Airworthiness Certificates, Required Documents, Marking & Registration
9.3 Welded Steel Tubular Structure: Splices, Sleeves & Engine Mount Repairs
Key Takeaways Explain This Topic AI
Welding on an engine mount, fuselage longeron, or truss member is an airframe major repair under Part 43 Appendix A(b)(1), which lists engine mounts and members of truss-type beams by name.
AC 43.13-1B Chapter 4 gives two accepted tube splice geometries: an inner sleeve driven inside the original tube, and an outer sleeve telescoped over the stubs of the original member.
An outer replacement tube telescoped over the original stubs is cut with a fishmouth at 30 degrees, which lengthens the weld bead and moves the heat-affected zone away from a single stress line.
A repaired member must be at least as strong as the original, so a sleeve is selected by wall thickness and material rather than by outside diameter alone.
The manufacturer's welded-repair data governs when it exists; AC 43.13-1B is acceptable data and cannot by itself approve a major structural weld repair for return to service.
Last updated: September 2026
9.3 Welded Steel Tubular Structure: Splices, Sleeves & Engine Mount Repairs
Warning
Every welded repair to primary structure is a major repair. Part 43 Appendix A(b)(1) classifies repairs "involving the strengthening, reinforcing, splicing, and manufacturing of primary structural members or their replacement" as airframe major repairs, and the enumerated list names members of truss-type beams (vi) , engine mounts (xii) , fuselage longerons (xiii) , and members of the side truss, horizontal truss, or bulkheads (xiv) . There is no such thing as a "minor weld" on a fuselage truss.
Steel tube structure is not a museum topic. Cubs, Champs, Huskies, Maules, Citabrias, and every certificated helicopter tail boom truss are welded 4130 steel, and the engine mount on a great many modern singles is a welded tube assembly. AC 43.13-1B Chapter 4 covers the accepted methods.
When Welding Is Acceptable at All
Three questions come before any geometry:
Does the manufacturer publish a repair for this member? If a structural repair manual or an FAA-approved repair scheme exists, it governs. AC 43.13-1B is acceptable data, not approved data, and cannot on its own substantiate a major repair (Section 5.1).
Is the member repairable, or must it be replaced? Heavily corroded, previously repaired, or heat-damaged tubing is often replaced rather than spliced.
Was the original member heat-treated? Welding on heat-treated 4130 changes its properties in the heat-affected zone. Repairs to heat-treated members generally require re-heat-treatment or an engineering-substantiated alternative.
The Two Splice Geometries
AC 43.13-1B Chapter 4 accepts two families of tube splice, and the exam distinguishes them by how the replacement material relates to the original tube.
Inner Sleeve (Insert Splice)
A tube of the same material , sized to slip inside the original tube, is inserted across the damaged joint and welded through prepared slots or at rosette welds. The outside contour of the member is preserved, which matters where the tube passes through fairings or where clearance is tight.
Outer Sleeve (Telescoped Splice)
A larger diameter replacement tube is telescoped over the stubs of the original member and welded in place. This is the geometry used when the damaged section is cut out entirely and a new center section is installed, and it is the geometry the IAR test asks about.
How is the replacement tube cut? With a fishmouth cut at 30 degrees . The reason is mechanical, not cosmetic:
A perpendicular (90-degree) cut puts the entire weld on one plane, concentrating the heat-affected zone and the stress riser on a single circumferential line.
A 45-degree diagonal cut improves that but still terminates in two sharp points.
The 30-degree fishmouth produces a long, gradually tapering weld line that distributes load transfer along the length of the joint and moves the end of the weld away from the point of maximum bending.
The same reasoning explains the alternative accepted geometry — a scarf cut — and explains why sleeve length matters: a splice sleeve must overlap enough of the parent tube to transfer the load through the weld rather than through the fit.
Selecting the Replacement Material
The governing standard is § 43.13(b): the repaired member must end up at least equal to its original condition with regard to structural strength. In practice that means:
Selection Criterion Rule of Thumb Why It Matters
Material Same alloy as the original (typically 4130 steel) Mixed alloys weld unpredictably and have different allowables
Wall thickness At least equal to the original; sleeves are commonly one gauge heavier The sleeve must carry the load the parent tube carried
Diameter Inner sleeve sized for a slip fit inside; outer sleeve sized for a slip fit over A loose fit means the weld carries load it was not designed to carry
Length Per the accepted splice geometry, long enough for load transfer Short sleeves fail at the weld toe
The exam frequently offers an answer that gets one of these right and another wrong — for instance, an outer sleeve of correct length but of thinner wall than the original. That answer is wrong on the § 43.13(b) standard alone.
Weld Quality: What the Inspector Looks For
The IA is inspecting someone else's weld, usually after the fact and often after paint. AC 43.13-1B Chapter 4 describes acceptable and unacceptable weld characteristics:
Acceptable weld indications:
- Uniform bead width and height with even ripple spacing
- Good penetration and fusion into the base metal at both toes
- Smooth tapering of the bead into the base metal
- No burning through or undercut of the parent tube
Rejectable weld indications:
- Undercut at the weld toe — a machined-in stress riser
- Lack of penetration or fusion — a joint held together by surface metal
- Excessive buildup with an abrupt transition — the load path steps rather than tapers
- Cracks anywhere in the weld or heat-affected zone
- Oxidation or scaling indicating excessive heat or inadequate shielding
- Evidence of welding over a previous weld without removing the old bead
A special watch item: a tube that has been welded and then filled, primed, and painted can conceal all of the above. Where the records show a welded repair to primary structure and the area has been refinished, the IA should require substantiating documentation of the repair scheme rather than judging the joint through the paint.
Corrosion in Steel Tube Structure
The failure mode that actually grounds steel tube airframes is not weld failure — it is internal corrosion , which is invisible from outside. Water enters through unsealed joints, drain holes, or cracked fabric and works from the inside out.
Lower longerons and cluster joints are the classic locations, because water settles there.
Sounding and probing the tube, inspecting through drain holes with a borescope, and checking for external rust blooms at cluster welds are the standard techniques.
A tube whose wall has been thinned by internal corrosion is not repairable by adding an external sleeve over the corroded region; the corroded material must be removed.
Documenting the Repair
Because a welded repair to a longeron, truss member, or engine mount is a major repair :
The work must be accomplished using approved data — manufacturer repair data, a DER-approved Form 8110-3, or a field approval (Section 5.1).
FAA Form 337 must be executed and disposed of under Part 43 Appendix B(a): duplicate copies, one signed copy to the owner, one to the FAA Aircraft Registration Branch within 48 hours after approval for return to service.
Item 8 must describe the repair specifically — which member, which station, what splice geometry, what material and wall thickness, and the exact approved data reference with revision and date.
Only an IA, an appropriately rated repair station, or the manufacturer may approve it for return to service.
High-Yield Exam Traps
The fishmouth cut is 30 degrees. Not 45, not 90.
Engine mounts are named in Appendix A(b)(1)(xii) — welding one is unambiguously a major repair.
A sleeve that is thinner than the original fails § 43.13(b) no matter how well it is welded.
AC 43.13-1B is acceptable data. A welded major repair still needs approved data and a Form 337.
Internal corrosion is the real killer in tube structure, and it cannot be sleeved over.