Study guide

Phase Diagrams and Alloy Systems

FE Fundamentals of Engineering Exam

Track your progress as you read

Finished sections get a check mark.

1 Introduction to the FE Exam

About the FE Exam FE Exam Study Strategies Navigating the FE Reference Handbook

2 Mathematics (8–12 Questions)

Analytic Geometry and Trigonometry Single-Variable Calculus Differential Equations Linear Algebra and Matrix Operations Numerical Methods

3 Probability and Statistics (6–9 Questions)

Probability Fundamentals Probability Distributions Statistical Estimation and Hypothesis Testing

4 Chemistry (5–8 Questions)

Chemical Reactions and Stoichiometry Acids, Bases, and pH Oxidation-Reduction and Corrosion

5 Ethics and Professional Practice (5–8 Questions)

Engineering Ethics Fundamentals

6 Engineering Economics (6–9 Questions)

Time Value of Money Economic Analysis Methods

7 Statics (9–14 Questions)

Force Systems and Equilibrium Trusses, Frames, and Machines Centroids and Moments of Inertia Static Friction

8 Dynamics (9–14 Questions)

Particle Kinematics Kinetics: Force, Mass, and Acceleration Work, Energy, Impulse, and Momentum Rigid-Body Rotation and Mechanical Vibrations

9 Strength of Materials (9–14 Questions)

Stress and Strain Fundamentals Beam Analysis: Shear and Moment Diagrams Bending Stress and Torsion Stress Transformation and Material Failure

10 Materials Science (6–9 Questions)

Material Properties and Selection Phase Diagrams and Alloy Systems

11 Fluid Mechanics (12–18 Questions)

Fluid Properties and Statics Fluid Dynamics and Bernoulli's Equation Pumps, Turbines, and Flow Measurement

12 Thermodynamics and Heat Transfer (9–14 Questions)

Laws of Thermodynamics and Properties Thermodynamic Cycles and Applications Heat Transfer: Conduction, Convection, and Radiation

13 Basic Electrical Engineering (6–9 Questions)

Electrical Fundamentals and DC Circuits AC Circuits and Three-Phase Power

14 Safety, Health, and Environment (6–9 Questions)

Industrial Safety and Hazard Management

15 Instrumentation and Controls (4–6 Questions)

Sensors, Data Acquisition, and Control Systems

16 Computational Tools and Computer Science

Spreadsheets, Structured Programming, and Flowcharts

Phase Diagrams and Alloy Systems

Key Takeaways Explain This Topic AI

A phase diagram maps which phases are stable at each temperature and composition; liquidus, solidus, and solvus are the key boundaries.

The lever rule gives phase fractions in a two-phase region: Wα = (Cβ − C₀)/(Cβ − Cα), using compositions at the ends of the tie line.

Invariant reactions: eutectic (L → α + β), eutectoid (γ → α + β), and peritectic (L + α → β).

The Fe–C diagram is central: steel is < 2.14% C, cast iron > 2.14% C; the eutectoid at 727 °C and 0.76% C forms pearlite.

Key Fe–C phases: ferrite (α, BCC, soft), austenite (γ, FCC), cementite (Fe₃C, 6.67% C, hard/brittle), martensite (BCT, from quenching).

Heat treatment tunes properties: annealing (soft), normalizing (refined grain), quenching (hard martensite), tempering (restores toughness).

Last updated: June 2026

Reading a Phase Diagram

A phase is a region of uniform composition and structure. A binary phase diagram plots temperature (y) versus composition (x) and shows which phase(s) are stable at any point.

  • Boundary/feature Meaning
  • Liquidus Above it, everything is liquid
  • Solidus Below it, everything is solid
  • Solvus Solid-solubility limit between two solid phases
  • Single-phase region One phase stable (α, β, L, γ)
  • Two-phase region Two phases coexist along a horizontal tie line
  • Invariant point Fixed T and composition where 3 phases coexist

Inside a two-phase region, the tie line's endpoints give the compositions of the two coexisting phases, and the lever rule gives their amounts.

The Lever Rule

For an overall composition C₀ inside a two-phase (α + β) field with tie-line ends at Cα and Cβ: W α = C β − C 0 C β − C α W β = C 0 − C α C β − C α W\alpha = \frac{C_\beta - C_0}{C_\beta - C\alpha} \qquad W_\beta = \frac{C_0 - C\alpha}{C_\beta - C\alpha} W α = C β ​ − C α C β ​ − C 0 ​ ​ W β ​ = C β ​ − C α C 0 ​ − C α ​

The fraction of a phase is proportional to the length of the tie line on the opposite side of C₀ (the "lever" balances about C₀).

Worked example: An alloy with overall composition C₀ = 40% B sits in a two-phase region with α at Cα = 20% B and β at Cβ = 60% B. Then Wβ = (40 − 20)/(60 − 20) = 20/40 = 0.50 , and Wα = (60 − 40)/(60 − 20) = 0.50 . The alloy is half α, half β. (Always subtract along the tie line — using temperatures instead of compositions is a classic mistake.)

Invariant Reactions

  • Reaction Transformation on cooling Example
  • Eutectic L → α + β Pb–Sn solder, 183 °C
  • Eutectoid γ → α + β Fe–C, 727 °C
  • Peritectic L + α → β Fe–C, 1,495 °C
  • The Gibbs Phase Rule

The Gibbs phase rule tells you how many variables you can change independently: P + F = C + 2 (or at constant pressure, P + F = C + 1), where P = number of phases, F = degrees of freedom, and C = number of components. In a binary (C = 2) diagram at fixed pressure, a single-phase region has F = 2 (temperature and composition both free), a two-phase region has F = 1, and an invariant point (three phases, like the eutectic) has F = 0 — temperature and all compositions are fixed, which is exactly why those reactions occur at a single sharp temperature.

The Iron–Carbon Diagram

The Fe–C (Fe–Fe₃C) diagram is the most important system in engineering practice.

  • Phase Structure Carbon Character
  • Ferrite (α) BCC ≤ 0.022% Soft, ductile, magnetic
  • Austenite (γ) FCC ≤ 2.14% Soft, ductile, non-magnetic
  • Cementite (Fe₃C) Orthorhombic 6.67% Very hard, brittle
  • Pearlite Lamellar α + Fe₃C 0.76% Moderate strength + ductility
  • Martensite BCT = parent γ Very hard, brittle (quenched)

Key points:

  • Point T C Reaction
  • Eutectoid 727 °C 0.76% γ → α + Fe₃C (pearlite)
  • Eutectic 1,147 °C 4.30% L → γ + Fe₃C
  • Max C in austenite 1,147 °C 2.14% Steel/cast-iron boundary

The 2.14% C line divides steels (workable, weldable) from cast irons (castable, brittle). Steels are graded by carbon: low-carbon/mild (< 0.25% C, ductile, weldable), medium-carbon (0.25–0.60% C, balanced), and high-carbon (0.60–2.14% C, hard, strong, less ductile). Alloys at exactly 0.76% C are eutectoid (fully pearlite); below that are hypoeutectoid (proeutectoid ferrite + pearlite); above are hypereutectoid (proeutectoid cementite + pearlite).

Heat Treatment

Heat treatment manipulates the microstructure predicted by the Fe–C diagram to set hardness, strength, and toughness.

  • Treatment Process Result
  • Annealing Heat above critical T, slow furnace cool Soft, ductile, stress-relieved, coarse pearlite
  • Normalizing Heat above critical T, air cool Refined grain, finer pearlite, moderate strength
  • Quenching Heat to austenite, rapid water/oil cool Hard, brittle martensite
  • Tempering Reheat quenched steel below critical T Trades some hardness for restored toughness
  • Case hardening Carburize/nitride the surface only Hard wear-resistant case, tough ductile core

Why quenching hardens: rapid cooling gives carbon atoms no time to diffuse out of the FCC austenite, trapping them in a strained body-centered tetragonal (BCT) martensite . The lattice distortion blocks dislocation motion, producing extreme hardness but brittleness — which is why quenched parts are almost always tempered afterward to recover toughness.

The quench → temper sequence is the cornerstone of producing tough, high-strength steel components (gears, shafts, tools). Annealing and normalizing, by contrast, are used when softness, machinability, or a uniform refined grain is the goal.

Hardenability — how deeply martensite forms on quenching — depends on alloying elements (Cr, Mo, Ni) and is measured by the Jominy end-quench test; it differs from hardness , which is just the surface indentation value of the final part.

The Lever Rule and Iron-Carbon Reactions

In a two-phase region of a binary phase diagram, the lever rule gives the mass fraction of each phase. Drawing a tie line at the temperature of interest, the fraction of one phase equals the opposite arm divided by the total tie-line length: f_liquid = (C₀−C_solid)/(C_liquid−C_solid).

  • Quantity Lever-rule expression
  • Fraction liquid (C₀ − C_s)/(C_l − C_s)
  • Fraction solid (C_l − C₀)/(C_l − C_s)

The iron-carbon diagram anchors steel metallurgy: the eutectoid reaction at 727°C and 0.76% C transforms austenite into pearlite (alternating ferrite + cementite). Steels below 0.76% C are hypoeutectoid; above, hypereutectoid. Heat treatments exploit this — slow cooling gives soft pearlite, while rapid quenching traps carbon as hard, brittle martensite , later softened by tempering. Knowing eutectic vs eutectoid (liquid→two solids vs solid→two solids) is a recurring FE distinction.