Study guide
11.2 Cracks — Causes & Prevention
IIW International Welding Inspector — Standard IWI-S
Track your progress as you read
Finished sections get a check mark.
1 Introduction & Exam Overview
1.1 About the IWI-S Qualification 1.2 Exam Structure, Routes & Scoring 1.3 How to Use This Guide
2 Inspector Role & Responsibilities
2.1 Inspector Duties Across the Weld Lifecycle 2.2 Reports, Traceability & Authority 2.3 IWI-S vs Basic and Comprehensive
3 Chapter 3: Arc Welding Processes I
3.1 Welding Technology Overview & Arc Fundamentals 3.2 MMA/SMAW Process & Flux-Coated Electrodes 3.3 MIG/MAG (GMAW) & Flux-Cored Arc Welding 3.4 TIG/GTAW Process
4 Chapter 4: Processes, Parameters & Consumables
4.1 SAW and Other Welding Processes 4.2 Cutting, Edge Preparation & Mechanisation 4.3 Heat Input, Arc Energy, Polarity & Parameters 4.4 ISO 4063 Process Numbers & Consumable Standards
5 Chapter 5: Metallurgy Foundations
5.1 Metals, Fe-C Alloys & Steel Classification 5.2 Structure of the Welded Joint & HAZ Zones 5.3 Carbon Equivalent, Hardenability & ISO/TR 15608 Groups
6 Chapter 6: Cracking Phenomena
6.1 Hydrogen Cold Cracking 6.2 Hot & Solidification Cracking 6.3 Lamellar Tearing 6.4 Fracture Types Related to Weld Defects
7 Chapter 7: Heat Treatment & Steel Families
7.1 Preheat, Interpass & PWHT 7.2 Carbon, Low-Alloy & Fine-Grain Steels 7.3 Creep-Resistant & Cryogenic Steels
8 Chapter 8: Stainless, Aluminium & Other Materials
8.1 Stainless & Heat-Resistant Steels 8.2 Aluminium & Aluminium Alloys 8.3 Nickel, Dissimilar Joints & Other Materials 8.4 Corrosion, Wear & Protective Layers
9 Chapter 9: Design & Welding Symbols
9.1 Strength of Materials Basics for Inspectors 9.2 Welded Joint Design & Preparation 9.3 ISO 2553 Welding Symbols 9.4 Fillet Throat Sizing & Structural Loading
10 Chapter 10: Fatigue, Distortion & Fabrication
10.1 Fatigue, Weld-Toe Effects & Fracture Mechanics Intro 10.2 Residual Stress & Distortion Control 10.3 Repair Welding, Plant Facilities & Health/Safety
11 Chapter 11: Weld Imperfections I
11.1 ISO 6520 Imperfection Classification 11.2 Cracks — Causes & Prevention 11.3 Porosity & Gas-Related Imperfections 11.4 Lack of Fusion & Lack of Penetration
12 Chapter 12: Weld Imperfections II
12.1 Undercut, Overlap & Shape Imperfections 12.2 Inclusions, Misalignment & Miscellaneous Defects 12.3 Evaluating Imperfections for Acceptance
13 Chapter 13: Surface NDT Methods
13.1 Visual Testing (ISO 17637) 13.2 Liquid Penetrant Testing (PT) 13.3 Magnetic Particle Testing (MT)
14 Chapter 14: Volumetric NDT & Destructive Tests
14.1 Radiographic Testing (RT) & Film Quality 14.2 Ultrasonic Testing (UT) 14.3 NDT Method Selection, IQI & ISO 9712 14.4 Destructive Testing of Welded Joints
15 Chapter 15: Codes, Acceptance & Qualification
15.1 ISO 5817 Quality Levels B/C/D 15.2 ISO 3834 Quality Requirements 15.3 WPS, WPQR & ISO 15614 15.4 Welder Qualification ISO 9606
16 Chapter 16: QA Documentation & Exam Strategy
16.1 Inspection Stages, ITPs & Hold Points 16.2 Materials Certificates, Traceability & In-Process Control 16.3 NCR, Reporting & QC Documents 16.4 Application of Standards & Practical Exam Strategy
11.2 Cracks — Causes & Prevention
Key Takeaways Explain This Topic AI
Cracks may occur in weld metal, HAZ, or parent metal and may be longitudinal, transverse, or crater cracks at terminations
Under ISO 5817 quality levels B, C, and D, cracks are typically not permitted
Causes link to metallurgy: hydrogen cold cracking, hot/solidification cracking, lamellar tearing, and alloy-specific mechanisms
Prevention combines low-hydrogen practice, preheat/interpass, chemistry and bead-shape control, restraint management, and proper crater fill
Detection uses VT plus PT/MT for surface cracks and UT (often preferred over RT) for many planar embedded cracks, with delayed NDT when specified
Last updated: July 2026
11.2 Cracks — Causes & Prevention
Quick Answer: Cracks are planar ruptures with sharp tips. They may sit in weld metal , HAZ , or parent metal , and may run longitudinal , transverse , or form crater cracks at stop ends. Under ISO 5817 , cracks are typically not permitted at quality levels B, C, and D . Causes link to Chapter 6 metallurgy (hydrogen cold cracking, hot/solidification cracking, lamellar tearing). Prevention is procedure-driven; detection uses VT plus surface and volumetric NDT as specified.
Module WI1.7–1.8 and exam-meta defect topics expect IWI-S candidates to classify crack locations and orientations, know that cracks are generally rejectable under common structural acceptance standards, connect causes to metallurgical mechanisms already studied, and choose appropriate detection methods.
Why Cracks Sit at the Top of Severity
Compared with rounded gas pores, a crack:
Concentrates stress at a sharp tip .
Can grow under static, cyclic (fatigue), or environmental loading.
Often connects surfaces or critical ligaments in pressure and structural joints.
Is treated as not permitted in ISO 5817 quality levels B/C/D for the usual crack categories listed.
Therefore the inspector’s first duty when a crack-like indication appears is conservative classification and hold —not “watch and wait” without engineering authority.
Location: Weld Metal, HAZ, Parent Metal
Location Typical mechanisms (link to Chapter 6) Inspector clues
Weld metal Hot/solidification cracking; sometimes hydrogen cracking in high-strength deposits; crater cracks at terminations Follows centreline or chevron patterns; crater cracks at stop/start
HAZ Hydrogen cold cracking; liquation cracking in susceptible alloys; reheat cracking in some creep-resistant steels Parallel to fusion line; toe/root HAZ; delayed timing for HICC
Parent metal Lamellar tearing (through-thickness); base-metal brittle fracture from arc strikes/notches Step-like or terrace morphology for lamellar tearing; associated with high through-thickness strain
Location drives root-cause investigation and repair strategy . Repairing a HAZ hydrogen crack without fixing hydrogen control is not a lasting solution.
Orientation and Morphology Terms
Longitudinal cracks run roughly parallel to the weld axis. Classic examples include solidification centreline cracks in deep, narrow beads and some hydrogen cracks aligned with residual longitudinal stress fields.
Transverse cracks run across the weld axis, often in weld metal or HAZ under longitudinal residual tension. They may appear as a series of short cracks.
Crater cracks form in the final solidification crater when the arc is broken without proper fill or down-slope. They are often star-shaped or short longitudinal remnants in the crater. Many procedures require crater fill , back-step, or controlled termination—and VT specifically checks stop ends.
Radiating / branching cracks and chevron patterns may indicate progressive fracture or solidification patterns; report morphology carefully for metallurgy follow-up.
Microfissures and hot-crack networks may be fine; still classify as crack-type imperfections when identified.
Hot Versus Cold (Recap for Imperfection Classification)
Use Chapter 6 mechanisms when writing NCRs:
Hot / solidification cracking — during the last stages of solidification; associated with wide freezing range, impurities (S, P), deep narrow beads, high dilution/restraint. Prevention: chemistry control, bead shape, parameter and sequence control.
Hydrogen cold cracking (HICC) — after cooling; needs hydrogen + hard microstructure + tensile stress + low temperature. Prevention: low-H consumables, dry storage, cleanliness, preheat/interpass, reduced restraint, delayed NDT when required.
Lamellar tearing — parent plate through-thickness weakness under high strain (T-joints, stiff node welds). Prevention: material selection (through-thickness properties), joint design, buttering, sequence.
Liquation / reheat — alloy-specific; recognise as specialist metallurgical issues for stainless, Ni alloys, and some creep steels (Chapters 7–8).
The ISO 6520 name may simply be “crack (longitudinal) in HAZ”; the cause narrative for the quality system uses the metallurgical category.
Acceptance: ISO 5817 Practice for Cracks
For steel fusion welds assessed to ISO 5817 :
Cracks (including microcracks in the usual tables) are not permitted at B, C, and D for the categories covered.
Do not apply “pore diameter logic” to cracks—there is no “small enough crack” under those tables for ordinary acceptance.
Product standards or client specs may be equal or stricter ; they rarely make structural cracks acceptable without formal engineering critical assessment (ECA), which is outside routine shop acceptance.
IWI-S rule of thumb for exams and practice: treat cracks as zero-tolerance under ISO 5817 B/C/D unless a documented ECA/fitness-for-purpose route is formally invoked by the contract—and that is not casual field discretion.
- Causes Checklist (Shop Floor)
- Consumable and hydrogen control
Damp basic electrodes, wet flux, contaminated wire.
Cellulosic electrodes on hardenable, restrained joints without justified procedure.
Oil, paint, moisture, and primers left in the weld zone.
Parameters and technique
Excessive depth-to-width ratio promoting centreline solidification cracks.
High dilution into sulphur-bearing parent metal.
Abrupt arc breaks creating crater cracks.
Excessive heat input or too-low heat input depending on mechanism (hot crack vs hard HAZ cold crack).
Design and restraint
High restraint fixtures, thick sections, rigid nodes.
Poor joint design promoting through-thickness strain (lamellar risk).
Repair welding in stiff structures without revised controls.
Material
High carbon equivalent / hardenable steels without preheat.
Segregation-prone compositions; poor through-thickness ductility plate.
Incorrect consumable matching for solidification cracking susceptibility.
Prevention Toolbox (Inspector Verification Focus)
- Prevention control What the inspector verifies
- WPS hydrogen strategy Consumable designation, baking/holding logs, issue times
- Preheat / interpass / post-heat Measured temperatures, locations, method
- Joint cleanliness Visual check before welding; coating removal in zone
- Termination practice Crater fill, run-off tabs, back-step as specified
- Bead placement / heat input Amperage, voltage, travel speed within WPS; bead shape
- Material suitability Certificates for through-thickness / chemistry when required
- Sequence and restraint Compliance with approved sequence; clamp practice
- Delayed NDT Hold time before final crack-sensitive inspection
- Detection Methods Overview
Visual testing (VT) — first line for surface-breaking cracks, crater cracks, toe cracks, and arc-strike cracks. Needs good lighting, access, and sometimes light grinding for profile assessment—without removing evidence prematurely when investigation is needed.
Liquid penetrant testing (PT) — surface-breaking cracks on non-magnetic and magnetic materials; excellent for stainless and non-ferrous. Cleanliness critical.
Magnetic particle testing (MT) — surface and slightly subsurface cracks in ferromagnetic materials; highly effective at toes and weld faces.
Radiographic testing (RT) — can show some cracks when oriented favourably to the beam, but tight, unfavourably oriented cracks may be missed. RT is stronger for volumetric rounded indications than for all planar cracks.
Ultrasonic testing (UT) — generally more sensitive to many planar crack-like flaws when properly applied and when geometry allows. Preferred volumetric method for many crack-sensitive butt welds in thick sections (method selection in Chapters 13–14).
Destructive tests — fracture faces, bend tests, and macro sections reveal cracks in procedure qualification and production cut-outs; not a production 100% tool.
Timing: for hydrogen cracking risk, respect delay before final NDT when specified—early clean NDT can be a false comfort.
Reporting and Disposition
Report:
Type — crack (and morphology if clear: longitudinal, transverse, crater).
Location — weld metal / HAZ / parent; surface / embedded; toe / root / centreline.
Dimensions — visible length; depth if known from NDT.
Method of detection and reference standard.
Acceptance statement — typically non-conforming to ISO 5817 level X.
Hold for engineering disposition / approved repair WPS.
Repairs must follow an approved repair procedure (often a repair WPS), with renewed NDT and, where applicable, renewed hydrogen controls and heat treatment.
Link Forward
Section 11.3 contrasts cracks with porosity , which is often limited rather than zero-tolerance. Section 11.4 covers other planar rejectables—lack of fusion and lack of penetration. Chapters 13–14 expand NDT capabilities and limitations. When cracks recur, reopen the Chapter 6 four-condition or solidification checklist rather than blaming only the last welder by default.