Study guide

13.3 Magnetic Particle Testing (MT)

IIW International Welding Inspector — Standard IWI-S

Track your progress as you read

Finished sections get a check mark.

1 Introduction & Exam Overview

1.1 About the IWI-S Qualification 1.2 Exam Structure, Routes & Scoring 1.3 How to Use This Guide

2 Inspector Role & Responsibilities

2.1 Inspector Duties Across the Weld Lifecycle 2.2 Reports, Traceability & Authority 2.3 IWI-S vs Basic and Comprehensive

3 Chapter 3: Arc Welding Processes I

3.1 Welding Technology Overview & Arc Fundamentals 3.2 MMA/SMAW Process & Flux-Coated Electrodes 3.3 MIG/MAG (GMAW) & Flux-Cored Arc Welding 3.4 TIG/GTAW Process

4 Chapter 4: Processes, Parameters & Consumables

4.1 SAW and Other Welding Processes 4.2 Cutting, Edge Preparation & Mechanisation 4.3 Heat Input, Arc Energy, Polarity & Parameters 4.4 ISO 4063 Process Numbers & Consumable Standards

5 Chapter 5: Metallurgy Foundations

5.1 Metals, Fe-C Alloys & Steel Classification 5.2 Structure of the Welded Joint & HAZ Zones 5.3 Carbon Equivalent, Hardenability & ISO/TR 15608 Groups

6 Chapter 6: Cracking Phenomena

6.1 Hydrogen Cold Cracking 6.2 Hot & Solidification Cracking 6.3 Lamellar Tearing 6.4 Fracture Types Related to Weld Defects

7 Chapter 7: Heat Treatment & Steel Families

7.1 Preheat, Interpass & PWHT 7.2 Carbon, Low-Alloy & Fine-Grain Steels 7.3 Creep-Resistant & Cryogenic Steels

8 Chapter 8: Stainless, Aluminium & Other Materials

8.1 Stainless & Heat-Resistant Steels 8.2 Aluminium & Aluminium Alloys 8.3 Nickel, Dissimilar Joints & Other Materials 8.4 Corrosion, Wear & Protective Layers

9 Chapter 9: Design & Welding Symbols

9.1 Strength of Materials Basics for Inspectors 9.2 Welded Joint Design & Preparation 9.3 ISO 2553 Welding Symbols 9.4 Fillet Throat Sizing & Structural Loading

10 Chapter 10: Fatigue, Distortion & Fabrication

10.1 Fatigue, Weld-Toe Effects & Fracture Mechanics Intro 10.2 Residual Stress & Distortion Control 10.3 Repair Welding, Plant Facilities & Health/Safety

11 Chapter 11: Weld Imperfections I

11.1 ISO 6520 Imperfection Classification 11.2 Cracks — Causes & Prevention 11.3 Porosity & Gas-Related Imperfections 11.4 Lack of Fusion & Lack of Penetration

12 Chapter 12: Weld Imperfections II

12.1 Undercut, Overlap & Shape Imperfections 12.2 Inclusions, Misalignment & Miscellaneous Defects 12.3 Evaluating Imperfections for Acceptance

13 Chapter 13: Surface NDT Methods

13.1 Visual Testing (ISO 17637) 13.2 Liquid Penetrant Testing (PT) 13.3 Magnetic Particle Testing (MT)

14 Chapter 14: Volumetric NDT & Destructive Tests

14.1 Radiographic Testing (RT) & Film Quality 14.2 Ultrasonic Testing (UT) 14.3 NDT Method Selection, IQI & ISO 9712 14.4 Destructive Testing of Welded Joints

15 Chapter 15: Codes, Acceptance & Qualification

15.1 ISO 5817 Quality Levels B/C/D 15.2 ISO 3834 Quality Requirements 15.3 WPS, WPQR & ISO 15614 15.4 Welder Qualification ISO 9606

16 Chapter 16: QA Documentation & Exam Strategy

16.1 Inspection Stages, ITPs & Hold Points 16.2 Materials Certificates, Traceability & In-Process Control 16.3 NCR, Reporting & QC Documents 16.4 Application of Standards & Practical Exam Strategy

13.3 Magnetic Particle Testing (MT)

Key Takeaways Explain This Topic AI

Magnetic particle testing (MT) applies only to ferromagnetic materials—typically carbon and low-alloy steels, not austenitic stainless or aluminium

Indications form where magnetic flux leaks at surface or near-surface discontinuities and magnetic particles accumulate

Magnetization methods include permanent/electromagnetic yokes, prods, and coils (among others); field direction relative to the discontinuity controls detectability

Dry particles suit rough/hot surfaces; wet particles (often fluorescent) suit smoother surfaces and higher sensitivity needs

Demagnetization and residual field limits matter for service and subsequent machining; inspectors review technique, coverage, and reports

Last updated: July 2026

13.3 Magnetic Particle Testing (MT)

Quick Answer: MT detects surface and near-surface discontinuities in ferromagnetic materials by flux leakage : magnetize the part, apply magnetic particles , and read accumulations at leaks. Yoke, prod, and coil methods are common. Austenitic stainless and aluminium cannot be MT-tested. Field direction should cut the expected crack path; demagnetize when required.

WI2.5 covers magnetic particle testing as a core surface NDT method for steel fabrication. For IWI-S, MT is often the default high-sensitivity surface method on carbon steel structures, pressure parts, and plant equipment— faster than PT for many shop welds, but useless on non-magnetic alloys.

Ferromagnetic Materials Only

MT requires the material to be capable of supporting a strong magnetic field and flux leakage at discontinuities. In welding inspection practice:

Material MT applicable?

  • Carbon steel, C-Mn steel Yes
  • Most low-alloy ferritic/martensitic steels Yes (procedure may note hardness/heat-treat state)
  • Duplex stainless (partially ferro) Procedure-specific — often limited/special
  • Austenitic stainless (e.g. 304/316 weldments) No (use PT/VT/other)
  • Aluminium, copper, titanium (non-ferro) No
  • Nickel alloys (generally non-ferro) No (exceptions rare/special)

Exam hammer: “Can we MT this 316L pipe weld?” → No —not ferromagnetic. Choose PT (or other methods) for surface cracks.

Some hardfacings, clad overlays, and dissimilar joints create mixed magnetic responses . The written procedure and NDT Level 3 guidance govern—not improvisation.

Flux Leakage Principle

When a ferromagnetic piece is magnetized , magnetic field lines travel preferentially through the metal. A discontinuity that interrupts the field—especially a crack roughly perpendicular to the field—forces flux to leak into the air above the surface. Fine magnetic particles applied to the surface are attracted to that leakage field and form a visible indication outlining the discontinuity.

Depth capability:

  • Surface-breaking discontinuities: highest sensitivity
  • Near-surface subsurface flaws: possible if shallow and properly oriented
  • Deep volumetric flaws: not an MT job—use UT/RT

Unlike PT, MT can find some near-surface flaws that are not open to the surface (tightly closed or slightly subsurface), provided flux leakage is strong enough. Paint or thin coatings may be allowed within procedure thickness limits; thick coatings kill sensitivity.

Orientation of Field vs Discontinuity

Maximum detectability occurs when the magnetic field is approximately perpendicular to the long axis of the discontinuity. A longitudinal crack may be missed if the field runs parallel to it.

Practical rule taught everywhere:

  • Magnetize in one direction and inspect
  • Magnetize in a roughly perpendicular second direction (or use multi-directional techniques where qualified)
  • Ensure overlap of magnetic field coverage along the weld length

For welds, expect cracks in various orientations (toe transverse, longitudinal centreline, crater). Two-directional coverage is standard unless a procedure justifies single-direction for a known single orientation risk.

  • Magnetization Methods — Overview
  • Electromagnetic yoke (AC/DC)
  • Portable legs placed across the weld; field between poles
  • AC yokes give good surface sensitivity and particle mobility; common for weld inspection

DC or permanent-magnet styles emphasize somewhat deeper near-surface capability with different particle behaviour—follow procedure

  • Lift-test / dead-weight checks verify yoke performance (procedure values)
  • Prods (current flow / direct contact)
  • Current injected through contact prods; field circles the current path

Useful on large structures; risk of arc strikes and local burning if poorly applied—inspectors watch for prod marks as imperfections

  • Spacing and amperage per procedure
  • Coils / cable wraps
  • Longitudinal magnetization of bars, shafts, pipes by coil
  • Flexible cables wrapped around vessels or pipes for circumferential field components depending on setup
  • More common in shop units and shaft inspection than every field weld, but concept appears in exams
  • Bench units / headshot–coil combinations
  • Production NDT of components with combined circular and longitudinal magnetization
  • Less central to site welding inspection but part of the MT method family

IWI-S focus: recognise yoke as the everyday weld tool; know prods and coils exist; demand two-direction coverage and calibrated equipment.

Dry vs Wet Particles

  • Feature Dry powder Wet (suspension)
  • Carrier Air-dusted powder Liquid bath or spray (water or oil vehicle)
  • Surface condition Better on hot , rough , outdoor steel Better on smoother surfaces
  • Sensitivity Good general Often higher for fine discontinuities (especially fluorescent wet)
  • Viewing Visible colour powders Visible or fluorescent under UV-A
  • Typical weld use Structural steel, as-welded profiles Critical shop welds, smoother ground toes

Fluorescent wet MT needs darkened viewing and UV checks similar in spirit to fluorescent PT. Colour contrast dry powders (grey, red, yellow) need good white light and colour contrast against the surface (sometimes a thin contrast paint is allowed by procedure).

Apply particles while the magnetizing force is applied (continuous method) or per residual method rules—procedure governs. Blowing dry powder gently avoids wiping away true indications.

  • Surface Preparation and Examination Zone
  • Remove loose scale, thick paint, weld spatter that prevents particle contact or creates false patterns
  • Thin adherent coatings: only if procedure permits a maximum thickness
  • Examine weld metal plus adjacent parent band as specified
  • Temperature limits apply for particles and for personnel safety on hot work
  • Demagnetization Notes

After MT, residual magnetism may:

  • Interfere with welding (arc blow) on subsequent passes or nearby work
  • Affect precision machining or instrumentation
  • Attract debris in service (rotating equipment, hydraulic parts)

Demagnetization (AC decay, reversing DC, yoke techniques, tunnel demag units) reduces residual field to procedure limits, sometimes verified with a field indicator or gauss meter. Not every structural weld requires demag after MT— service specification and procedure decide. Critical rotating parts and many shop procedures do require it. Know that residual field is a real close-out item, not optional folklore.

Limitations and Common Traps

  • Limitation Implication
  • Non-ferromagnetic metals Use PT/other—not MT
  • Field parallel to crack Missed indication—need second direction
  • Deep internal flaws UT/RT required
  • Excessively rough geometry Non-relevant particle traps
  • Prod burns New imperfections introduced by NDT
  • Over-magnetization / poor technique Heavy background, false calls
  • Thick coatings Reduced or zero sensitivity

False sense of security: MT “clean” on only one field direction along a long seam is incomplete technique, not a quality miracle.

Inspector Review of MT Work and Reports

Parallel to PT review, check:

Correct method selection (ferro material confirmed)

Procedure and acceptance standard (e.g. ISO 17638 principles + ISO 23278 acceptance levels, or ASME/client equivalents—use the contract edition)

  • Equipment verification (yoke lift test, UV meters if fluorescent, ammeter for prods)
  • Two-directional magnetization / multi-directional coverage and overlap
  • Particle type (dry/wet, visible/fluorescent) suited to surface and temperature
  • Examination extent and weld identification
  • Indications listed with sketch/photo as required; relevant vs non-relevant rationale
  • Demagnetization and residual field check when specified
  • Post-clean if contrast paint or wet particles must be removed before coating/service
  • Personnel qualification (ISO 9712 MT Level as required)
  • MT vs PT — Decision Table for Inspectors
  • Question Prefer
  • Carbon steel, as-welded, need fast surface crack screen MT (yoke) often
  • Austenitic stainless or aluminium PT
  • Need open-to-surface only confirmation on non-ferro PT
  • Slightly subsurface crack in ferro parent MT may work; confirm with procedure
  • Geometry too complex for field control Reassess access; may need PT or other
  • Hot surface rough steel Dry MT often preferred
  • Integration with VT and the ITP

Typical flow on a steel butt weld requiring surface NDT:

  • VT final geometry and cleanliness
  • MT (or PT) for surface/near-surface cracks per ITP
  • UT or RT if volumetric examination is specified
  • Repair loop: excavate → weld repair → re-VT → re-MT/PT → re-volumetric as required

IWI-S ensures hold points are real, sequences are logical (do not coat before MT when MT is required bare), and reports match the physical work.

  • High-Yield Summary for Oral/Written Exams
  • MT = ferromagnetic + flux leakage + particles
  • Not for austenitic SS / Al
  • Field ⟂ crack for best detection; two directions
  • Yoke / prod / coil families
  • Dry vs wet , visible vs fluorescent
  • Demagnetize when required
  • Review reports like a supervisor, not a spectator