Study guide
14.3 Casting Processes, Metal Forming & Welding Metallurgy
Coal India Management Trainee CIL MT
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: CIL MT Exam Overview & Coal Sector Landscape
1.1 CIL MT Exam Pattern, Marking Scheme & Strategy 1.2 Coal India Limited: Corporate Structure, Maharatna Status & Subsidiaries 1.3 Indian Coal Mining Sector, Energy Mix & Environmental Regulations
2 Chapter 2: Paper-I General Awareness, Polity & Current Affairs
2.1 Indian Constitution, Governance & Statutory Bodies 2.2 Indian Economy, Union Budget & Economic Planning 2.3 Indian Geography, Mineral Belts & Environmental Ecology 2.4 Modern Indian History, Freedom Struggle & Cultural Heritage 2.5 General Science: Physics, Chemistry & Biology Fundamentals 2.6 Inventions, Discoveries & Scientific-Technological Development 2.7 Uses of Internet, Computer Awareness & Digital Governance 2.8 National & International Organisations 2.9 Awards, Honours & Sports 2.10 Books & Authors, Important Monuments & Places of India 2.11 Ports, Power Plants & Infrastructure of India 2.12 Climate Change, SDGs, National Parks & Wildlife Sanctuaries 2.13 Flagship Government Programmes & Current Affairs Method 2.14 World Physical, Social & Economic Geography
3 Chapter 3: Paper-I Reasoning & Logical Ability
3.1 Series Completion, Coding-Decoding & Semantic Analogies 3.2 Syllogisms, Logical Deduction & Venn Diagrams 3.3 Seating Arrangements, Linear/Circular Alignments & Puzzles 3.4 Direction Sense, Blood Relations & Order/Ranking 3.5 Alphabetical & Alphanumeric Series 3.6 Statement & Conclusions, Statement & Arguments 3.7 Clocks & Calendars 3.8 Cubes, Dice & Figure Counting 3.9 Mirror Images, Water Images, Embedded Figures & Non-Verbal Series 3.10 Decision Making & Data Analysis in Reasoning
4 Chapter 4: Paper-I Numerical Ability & Quantitative Aptitude
4.1 Arithmetic Foundations: Percentages, Profit & Loss, Ratio & Proportion 4.2 Averages, Simple/Compound Interest, Alligations & Mixtures 4.3 Time & Work, Pipes & Cisterns, Time, Speed & Distance 4.4 Algebra, Mensuration, Geometry & Data Interpretation (DI) 4.5 Number System, LCM, HCF & Decimal Fractions 4.6 Surds, Indices & Simplification 4.7 Problems on Ages 4.8 Boats & Streams and Problems on Trains 4.9 Permutations & Combinations 4.10 Probability for Quantitative Aptitude
5 Chapter 5: Paper-I General English & Verbal Ability
5.1 English Grammar, Error Spotting & Sentence Correction 5.2 Vocabulary Building: Synonyms, Antonyms, Idioms & Phrases 5.3 Reading Comprehension, Cloze Tests & Para Jumbles 5.4 Fill in the Blanks, Cloze Passages & Sentence Completion 5.5 Jumbled Sentences & Sentence Improvement
6 Chapter 6: Paper-II Engineering Mathematics
6.1 Matrix Algebra, Rank & Systems of Linear Equations 6.2 Eigenvalues, Eigenvectors & the Cayley-Hamilton Theorem 6.3 Limits, Continuity, Differentiability & Mean Value Theorems 6.4 Maxima-Minima, Indeterminate Forms & Taylor Series 6.5 Definite, Improper, Double & Triple Integrals 6.6 Partial Derivatives, Total Derivative & Multivariable Optimisation 6.7 First-Order Differential Equations: Linear & Non-Linear 6.8 Higher-Order Linear Differential Equations & Engineering Applications 6.9 Laplace Transforms & Transfer-Function Methods 6.10 Probability, Conditional Probability & Bayes' Theorem 6.11 Random Variables, Distributions & Descriptive Statistics 6.12 Numerical Methods: Root Finding, Integration & ODE Solvers
7 Chapter 7: Paper-II Engineering Mechanics & Statics-Dynamics
7.1 Force Systems, Coplanar Equilibrium & Lami's Theorem 7.2 Plane Trusses, Friction Mechanics & Screws/Wedges 7.3 Centroids, Center of Gravity & Moment of Inertia 7.4 Kinematics, Kinetics of Particles & Rigid Body Dynamics 7.5 Virtual Work & Lagrange's Equation 7.6 Rolling Friction, Belt-Pulley Drives, Brakes, Clutches & Vehicle Dynamics
8 Chapter 8: Paper-II Mechanics of Materials & Structural Integrity
8.1 Simple Stresses, Strains, Elastic Moduli & Thermal Stresses 8.2 Principal Stresses, Strain Energy & Mohr's Circle 8.3 Shear Force & Bending Moment Diagrams, Beam Bending & Shear Stresses 8.4 Torsion of Circular Shafts, Springs & Column Buckling 8.5 Thin Cylinders, Spheres & Thick-Walled Pressure Vessels 8.6 Deflection of Beams: Double Integration, Macaulay & Moment-Area 8.7 Shear Centre & Unsymmetrical Bending 8.8 Strain Gauges, Rosettes & Experimental Stress Analysis 8.9 Mechanical Testing: Universal Testing Machine, Hardness & Impact
9 Chapter 9: Paper-II Theory of Machines & Mechanical Vibrations
9.1 Simple Mechanisms, Kinematic Inversions & Velocity/Acceleration Diagrams 9.2 Cams & Followers, Toothed Gearing & Epicyclic Gear Trains 9.3 Flywheels, Centrifugal/Inertia Governors & Rotor Balancing 9.4 Free, Damped & Forced Single-Degree-of-Freedom Vibrations 9.5 Gyroscopic Couple & Gyroscopic Effects
10 Chapter 10: Paper-II Machine Design & Failure Theories
10.1 Static Failure Theories & Variable/Fatigue Loading 10.2 Design of Threaded Fasteners, Welded & Riveted Joints 10.3 Design of Shafts, Keys, Couplings & Rolling/Sliding Bearings 10.4 Design of Spur, Helical, Bevel & Worm Gears 10.5 Design of Helical, Leaf & Torsion Springs 10.6 Design of Brakes & Clutches: Energy, Lining Pressure & Heat
11 Chapter 11: Paper-II Fluid Mechanics & Hydraulic Machinery
11.1 Fluid Properties, Hydrostatic Forces & Buoyancy 11.2 Fluid Kinematics, Continuity & Bernoulli's Equation 11.3 Viscous Flow in Pipes, Boundary Layer & Minor Losses 11.4 Hydraulic Turbines, Centrifugal & Reciprocating Pumps 11.5 Dimensional Analysis, Similitude & Model Testing 11.6 Control-Volume Analysis: Continuity, Momentum & Energy
12 Chapter 12: Paper-II Thermodynamics, Thermal Cycles & Turbomachinery
12.1 Fundamental Concepts, First & Second Laws of Thermodynamics 12.2 Entropy, Availability, Exergy & Properties of Pure Substances 12.3 Air-Standard Gas Power Cycles: Otto, Diesel, Dual & Brayton 12.4 Vapour Power Cycles: Ideal, Reheat & Regenerative Rankine Cycles 12.5 Thermodynamic Relations: Maxwell, Clausius-Clapeyron & Joule-Thomson 12.6 Behaviour of Ideal & Real Gases and Equations of State 12.7 Air & Gas Compressors: Reciprocating, Rotary & Multi-Stage 12.8 Steam & Gas Turbines: Impulse, Reaction & Velocity Diagrams
13 Chapter 13: Paper-II Heat Transfer, Refrigeration & Air Conditioning
13.1 Steady & Unsteady Conduction, Extended Surfaces (Fins) 13.2 Forced/Natural Convection, Radiation & Heat Exchanger LMTD/NTU 13.3 Vapour Compression & Vapour Absorption Refrigeration Systems 13.4 Psychrometric Properties, Processes & Air Conditioning Systems 13.5 Gas Refrigeration, Heat Pump Cycles & Cryogenics
14 Chapter 14: Paper-II Materials Science, Metallurgy & Manufacturing Technology
14.1 Crystal Structures, Phase Diagrams & Iron-Iron Carbide Equilibrium 14.2 Heat Treatment Processes & Engineering Alloy Steels 14.3 Casting Processes, Metal Forming & Welding Metallurgy 14.4 Metal Cutting Mechanics, Tool Life & Machine Tools 14.5 Plastic Deformation, Yield Criteria & Load Estimation in Bulk Forming 14.6 Sheet Metal Forming: Shearing, Bending & Deep Drawing 14.7 Powder Metallurgy 14.8 Brazing, Soldering & Adhesive Bonding 14.9 Non-Traditional Machining: EDM, ECM, USM, AJM, LBM & EBM 14.10 Abrasive Machining, Grinding & Superfinishing 14.11 Principles of Work Holding, Jigs & Fixtures 14.12 Economics of Machining & Tool Life Optimisation
15 Chapter 15: Paper-II Metrology, Quality Control & Industrial Engineering / OR
15.1 Limits, Fits, Tolerances, Gauges & Surface Metrology 15.2 Production Planning, Forecasting & Inventory Control Models 15.3 Operations Research: Linear Programming & Transportation/Assignment 15.4 Project Management: CPM, PERT, Network Analysis & Crashing 15.5 Comparators & Interferometry 15.6 Coordinate Measuring Machines & Machine Tool Alignment Testing 15.7 Computer Integrated Manufacturing: CAD/CAM & Integration Tools 15.8 NC/CNC Machines & CNC Part Programming 15.9 Material Requirements Planning, Scheduling & Sequencing 15.10 Queuing Theory & Simple Queuing Models 15.11 Network Flow Models: Shortest Route, Maximal Flow & Spanning Tree
14.3 Casting Processes, Metal Forming & Welding Metallurgy
Key Takeaways Explain This Topic AI
Pattern allowances account for solid contraction, mold taper (draft), machining finish, distortion, and rapping, while liquid and solidification shrinkage are compensated strictly by risers.
Chvorinov's solidification rule (ts = B*(V/A)^2) and the modulus method (M_riser >= 1.2 M_casting) govern progressive directional solidification into risers.
Metal forming mechanics dictate maximum roll draft (Delta_h_max = mu^2 * R), maximum bite angle (tan(alpha) <= mu), and theoretical maximum single-pass wire drawing reduction (63.2%).
Welding metallurgy involves heat generation (H = I^2 R t in spot welding), flame chemistry in oxy-acetylene welding, and heat-affected zone (HAZ) grain coarsening and hydrogen-induced cold cracking.
Last updated: August 2026
13.3 Casting Processes, Metal Forming & Welding Metallurgy
Manufacturing technology transforms raw engineering materials into functional components through solid-state casting, plastic deformation, and fusion joining. In mining engineering and plant construction, heavy cast gearboxes, forged turbine shafts, extruded pipeline sections, and welded structural frames must meet rigorous metallurgical and dimensional integrity standards.
1. Sand Casting Engineering & Pattern Design
Casting involves pouring molten metal into a refractory mold cavity containing the negative geometry of the desired part. [ Pouring Basin ]
- │
- [ Downsprue ] (Tapered to prevent air aspiration)
- │
- [ Sprue Well ]
- │
- [ Runner ] ─── [ Ingate ] ───> [ Mold Cavity ] ───> [ Riser ]
- Pattern Allowances
Patterns are enlarged or modified representations of the final casting, incorporating five critical allowances:
Shrinkage Allowance: Metals undergo three distinct stages of volumetric contraction:
Liquid Contraction (Pouring temp → \to → Freezing temp): Compensated by the riser .
Solidification Shrinkage (Liquid → \to → Solid phase change): Compensated by the riser .
Solid Contraction (Solid freezing temp → \to → Room temp): Compensated by enlarging pattern dimensions .
Typical solid shrinkage values: Steel ( 2.0 % = 20 mm/m 2.0\% = 20\text{ mm/m} 2.0% = 20 mm/m ), Cast Iron ( 1.0 % = 10 mm/m 1.0\% = 10\text{ mm/m} 1.0% = 10 mm/m , gray iron can expand during graphite precipitation), Aluminum ( 1.3 – 1.5 % = 13 – 15 mm/m 1.3\text{--}1.5\% = 13\text{--}15\text{ mm/m} 1.3 – 1.5% = 13 – 15 mm/m ), Brass ( 1.5 % = 15 mm/m 1.5\% = 15\text{ mm/m} 1.5% = 15 mm/m ), Invar ( 0 % 0\% 0% ).
Draft (Taper) Allowance: Vertical pattern surfaces are tapered by 1 ∘ to 3 ∘ 1^{\circ}\text{ to }3^{\circ} 1 ∘ to 3 ∘ ( 15 – 25 mm/m 15\text{--}25\text{ mm/m} 15 – 25 mm/m ) to permit withdrawal without damaging sand cavity walls.
Machining (Finish) Allowance: Additional stock ( 1.5 – 5.0 mm 1.5\text{--}5.0\text{ mm} 1.5 – 5.0 mm ) provided on mating surfaces to be cleaned up by machining.
Distortion (Camber) Allowance: Provided on U-shaped, V-shaped, or unequal-thickness castings that warp due to differential cooling stresses.
Rapping (Shake) Allowance: A negative allowance subtracted from pattern dimensions to compensate for cavity enlargement during mold rapping.
Gating System Dynamics
To prevent air aspiration in the vertical downsprue, the sprue must be parabolically or linearly tapered following the continuity and Bernoulli equations: A 1 h 1 = A 2 h 2 ⟹ A 1 A 2 = h 2 h 1 A_1 \sqrt{h_1} = A_2 \sqrt{h_2} \implies \frac{A_1}{A_2} = \sqrt{\frac{h_2}{h_1}} A 1 h 1 = A 2 h 2 ⟹ A 2 A 1 = h 1 h 2
Gating Ratio: The ratio of cross-sectional areas: Sprue Area ( A s ) : Runner Area ( A r ) : Total Ingate Area ( A g ) \text{Sprue Area } (A_s) : \text{Runner Area } (A_r) : \text{Total Ingate Area } (A_g) Sprue Area ( A s ) : Runner Area ( A r ) : Total Ingate Area ( A g ) .
Pressurized Gating ( 1 : 2 : 1 1 : 2 : 1 1 : 2 : 1 or 1 : 0.75 : 0.5 1 : 0.75 : 0.5 1 : 0.75 : 0.5 ): Choke area is at the ingate. High discharge velocity, full gating system, turbulent flow; suitable for ferrous alloys (cast iron, steel).
Unpressurized Gating ( 1 : 2 : 2 1 : 2 : 2 1 : 2 : 2 or 1 : 2 : 4 1 : 2 : 4 1 : 2 : 4 ): Choke area is at the sprue base. Low exit velocity, laminar filling, minimal oxide/dross entrapment; essential for aluminum, magnesium, and copper alloys.
- 2. Solidification Kinetics & Riser Design
- Chvorinov's Rule of Solidification
The total solidification time t s t_s t s of a casting is governed by its geometric modulus ( M = V / A M = V/A M = V / A ): t s = B ( V A ) n = B ⋅ M 2 ( with n = 2 ) t_s = B \left(\frac{V}{A}\right)^n = B \cdot M^2 \quad (\text{with } n = 2) t s = B ( A V ) n = B ⋅ M 2 ( with n = 2 )
where V V V is casting volume, A A A is heat dissipating surface area, and B B B is the mold constant (depending on metal latent heat, density, pouring temperature, and mold thermal diffusivity).
Modulus Method of Riser Design
To ensure directional solidification and feed liquid shrinkage, the riser must solidify after the casting: t s , riser ≥ t s , casting ⟹ M riser ≥ 1.2 ⋅ M casting t_{s, \text{riser}} \ge t_{s, \text{casting}} \implies M_{\text{riser}} \ge 1.2 \cdot M_{\text{casting}} t s , riser ≥ t s , casting ⟹ M riser ≥ 1.2 ⋅ M casting Optimum Top Riser ( h = d / 2 ) : M riser = V A = π 4 d 2 h π 4 d 2 + π d h = d 6 \text{Optimum Top Riser } (h = d/2): \quad M_{\text{riser}} = \frac{V}{A} = \frac{\frac{\pi}{4}d^2 h}{\frac{\pi}{4}d^2 + \pi d h} = \frac{d}{6} Optimum Top Riser ( h = d /2 ) : M riser = A V = 4 π d 2 + π d h 4 π d 2 h = 6 d Optimum Side Riser ( h = d ) : M riser = V A = π 4 d 3 2 ( π 4 d 2 ) + π d 2 = d 6 \text{Optimum Side Riser } (h = d): \quad M_{\text{riser}} = \frac{V}{A} = \frac{\frac{\pi}{4}d^3}{2\left(\frac{\pi}{4}d^2\right) + \pi d^2} = \frac{d}{6} Optimum Side Riser ( h = d ) : M riser = A V = 2 ( 4 π d 2 ) + π d 2 4 π d 3 = 6 d
Worked Step-by-Step Numerical Example
Problem: Compare the solidification times of three castings of equal volume V 0 V_0 V 0 : (a) a Sphere of diameter D D D , (b) a Cube of side a a a , and (c) a Cylinder with height equal to diameter ( h = d h = d h = d ).
Sphere: V 0 = π 6 D 3 ⟹ D = ( 6 V 0 π ) 1 / 3 V_0 = \frac{\pi}{6}D^3 \implies D = \left(\frac{6V_0}{\pi}\right)^{1/3} V 0 = 6 π D 3 ⟹ D = ( π 6 V 0 ) 1/3 . Surface area A = π D 2 = ( 36 π V 0 2 ) 1 / 3 ≈ 4.836 V 0 2 / 3 A = \pi D^2 = (36\pi V_0^2)^{1/3} \approx 4.836 V_0^{2/3} A = π D 2 = ( 36 π V 0 2 ) 1/3 ≈ 4.836 V 0 2/3 . Modulus M sphere = D 6 = 0.2068 V 0 1 / 3 M_{\text{sphere}} = \frac{D}{6} = 0.2068 V_0^{1/3} M sphere = 6 D = 0.2068 V 0 1/3 .
Cube: V 0 = a 3 ⟹ a = V 0 1 / 3 V_0 = a^3 \implies a = V_0^{1/3} V 0 = a 3 ⟹ a = V 0 1/3 . Surface area A = 6 a 2 = 6.000 V 0 2 / 3 A = 6a^2 = 6.000 V_0^{2/3} A = 6 a 2 = 6.000 V 0 2/3 . Modulus M cube = a 6 = 0.1667 V 0 1 / 3 M_{\text{cube}} = \frac{a}{6} = 0.1667 V_0^{1/3} M cube = 6 a = 0.1667 V 0 1/3 .
Cylinder ( h = d h=d h = d ): V 0 = π 4 d 3 ⟹ d = ( 4 V 0 π ) 1 / 3 V_0 = \frac{\pi}{4}d^3 \implies d = \left(\frac{4V_0}{\pi}\right)^{1/3} V 0 = 4 π d 3 ⟹ d = ( π 4 V 0 ) 1/3 . Surface area A = 3 π 2 d 2 ≈ 5.536 V 0 2 / 3 A = \frac{3\pi}{2}d^2 \approx 5.536 V_0^{2/3} A = 2 3 π d 2 ≈ 5.536 V 0 2/3 . Modulus M cyl = d 6 = 0.1806 V 0 1 / 3 M_{\text{cyl}} = \frac{d}{6} = 0.1806 V_0^{1/3} M cyl = 6 d = 0.1806 V 0 1/3 . Ratio of Solidification Times: t sphere : t cyl : t cube = ( 0.2068 ) 2 : ( 0.1806 ) 2 : ( 0.1667 ) 2 = 1.54 : 1.17 : 1.00 \text{Ratio of Solidification Times: } \quad t_{\text{sphere}} : t_{\text{cyl}} : t_{\text{cube}} = (0.2068)^2 : (0.1806)^2 : (0.1667)^2 = 1.54 : 1.17 : 1.00 Ratio of Solidification Times: t sphere : t cyl : t cube = ( 0.2068 ) 2 : ( 0.1806 ) 2 : ( 0.1667 ) 2 = 1.54 : 1.17 : 1.00
(Conclusion: The Sphere possesses the lowest surface area per unit volume, maximum modulus, and takes the longest time to solidify).
3. Advanced & Special Casting Processes
Investment Casting (Lost-Wax): Precision disposable wax pattern coated with refractory ceramic slurry, autoclave dewaxed, fired at 1000 ∘ C 1000^{\circ}\text{C} 100 0 ∘ C , poured, and broken. Unmatched surface finish ( 1.6 μ m 1.6\;\mu\text{m} 1.6 μ m ), intricate geometry, used for single-crystal gas turbine blades.
Die Casting: Liquid metal injected into permanent tool steel dies under high pressure ( 20 – 150 MPa 20\text{--}150\text{ MPa} 20 – 150 MPa ).
Hot Chamber: Injection plunger submerged in molten metal; rapid cycle; restricted to low-melting alloys (Zn, Pb, Mg) because molten Al erodes ferrous plungers.
Cold Chamber: Molten metal ladled into cold shot chamber; used for Al, Cu, and brass alloys.
Centrifugal Casting: Molten metal poured into a mold rotating at high speed ( G -factor = ω 2 R g ≈ 60 – 80 G\text{-factor} = \frac{\omega^2 R}{g} \approx 60\text{--}80 G -factor = g ω 2 R ≈ 60 – 80 ). True centrifugal casting produces hollow seamless pipes without internal cores; slag and low-density oxides float to the inner bore and are machined away.
Continuous Casting: Molten metal feeds continuously through a water-cooled oscillating copper mold to produce endless billets, blooms, and slabs ( > 95 % >95\% > 95% of modern primary steel production).
4. Metal Forming Mechanics
Plastic deformation occurs when applied mechanical stresses exceed the material's yield strength, governed by the flow curve (Hollomon power law): σ = K ε n \sigma = K \varepsilon^n σ = K ε n
where σ \sigma σ is true stress, ε = ln ( A 0 / A f ) \varepsilon = \ln(A_0/A_f) ε = ln ( A 0 / A f ) is true strain, K K K is strength coefficient, and n n n is strain hardening exponent. Flat Rolling Mechanics
- Roll Radius (R)
- ┌───────┐
- h0 (Initial) │ (•) ->│ v_r h1 (Final)
- ───────────────────┘ └───────────────────
- Entry (v0 < vr) Neutral Point Exit (vf > vr)
- ───────────────────┐ ┌───────────────────
- │ (•) <-│ v_r
- └───────┘
- Rolling Mechanics & Limiting Parameters
Draft ( Δ h \Delta h Δ h ): Reduction in plate thickness: Δ h = h 0 − h 1 \Delta h = h_0 - h_1 Δ h = h 0 − h 1 .
Maximum Angle of Bite without External Push: tan α ≤ μ ⟹ α max = arctan ( μ ) \tan\alpha \le \mu \implies \alpha_{\max} = \arctan(\mu) tan α ≤ μ ⟹ α m a x = arctan ( μ ) .
Maximum Single-Pass Draft: Δ h max = μ 2 R \Delta h_{\max} = \mu^2 R Δ h m a x = μ 2 R
Neutral (No-Slip) Point: The specific point along the roll-strip contact arc where strip velocity equals the horizontal component of roll peripheral speed ( v = v r cos θ v = v_r \cos\theta v = v r cos θ ).
Forward Slip ( S f S_f S f ): S f = v f − v r v r × 100 % S_f = \frac{v_f - v_r}{v_r} \times 100\% S f = v r v f − v r × 100% .
Extrusion & Wire Drawing Mechanics
Direct (Forward) Extrusion: Billet slides against container walls; heavy friction causes high initial peak pressure, decaying as stroke progresses.
Indirect (Backward) Extrusion: Die moves into stationary billet; zero relative motion between billet and container; constant extrusion pressure, ∼ 25 – 30 % \sim 25\text{--}30\% ∼ 25 – 30% lower force requirement.
Wire Drawing Maximum Theoretical Single-Pass Reduction: Under ideal plastic deformation without friction or redundant shear work: σ d = σ 0 ln ( A 0 A f ) ≤ σ 0 ⟹ ln ( A 0 A f ) ≤ 1 ⟹ A f A 0 = 1 e ≈ 0.3679 \sigma_d = \sigma_0 \ln\left(\frac{A_0}{A_f}\right) \le \sigma_0 \implies \ln\left(\frac{A_0}{A_f}\right) \le 1 \implies \frac{A_f}{A_0} = \frac{1}{e} \approx 0.3679 σ d = σ 0 ln ( A f A 0 ) ≤ σ 0 ⟹ ln ( A f A 0 ) ≤ 1 ⟹ A 0 A f = e 1 ≈ 0.3679 R max = 1 − A f A 0 = 1 − 1 e = 1 − 0.3679 = 0.6321 ⟹ 63.21 % R_{\max} = 1 - \frac{A_f}{A_0} = 1 - \frac{1}{e} = 1 - 0.3679 = 0.6321 \implies 63.21\% R m a x = 1 − A 0 A f = 1 − e 1 = 1 − 0.3679 = 0.6321 ⟹ 63.21%
- 5. Welding Processes & Welding Metallurgy Oxy-Acetylene Flame Types
- Neutral (1:1) [Inner Cone 3200°C]=====[Outer Envelope]======>
- Oxidizing (1.5:1) [Pointed Sharp Cone 3400°C]===[Short Envelope]=>
- Carburizing (0.9:1) [Inner Cone]==[Acetylene Feather 3000°C]==[Outer Envelope]=>
- Welding Process Fundamentals
Shielded Metal Arc Welding (SMAW): Consumable flux-coated stick electrode provides protective CO 2 \text{CO}_2 CO 2 gas shield, deoxidizers, and slag cover.
Gas Tungsten Arc Welding (GTAW / TIG): Non-consumable tungsten electrode + inert Argon/Helium shield. Direct Current Electrode Negative ( DCEN ) provides 70 % 70\% 70% heat at workpiece (deep penetration). Direct Current Electrode Positive ( DCEP ) or AC provides cathodic cleaning to break refractory Al 2 O 3 \text{Al}_2\text{O}_3 Al 2 O 3 films on aluminum alloys.
Gas Metal Arc Welding (GMAW / MIG): Continuous consumable wire electrode; modes of transfer include short-circuiting, globular, spray (requires high current + Ar shield), and pulsed spray.
Submerged Arc Welding (SAW): Arc is fully buried beneath a blanket of granular fusible flux; zero spatter, ultra-high current ( > 1000 A >1000\text{ A} > 1000 A ) and deposition rates; restricted to 1 G / 1 F 1\text{G}/1\text{F} 1 G /1 F flat positions.
Resistance Spot Welding (RSW): Joule heating at contact interface: H = I 2 R t H = I^2 R t H = I 2 Rt
Because faying surface contact resistance R contact R_{\text{contact}} R contact is highest, the molten weld nugget nucleates precisely at the sheet interface.
Heat-Affected Zone (HAZ) & Weld Defects [ Base Metal ] ───> [ Subcritical HAZ ] ───> [ Intercritical ] ───> [ Coarse Grain HAZ ] ───> [ Weld Fusion Zone ]
(Unaltered) (Stress Relieved) (Fine Grain α+γ) (>1100°C, Brittle Martensite) (Cast Dendrites)
Coarse Grain HAZ: Peak temperatures > 1100 ∘ C >1100^{\circ}\text{C} > 110 0 ∘ C induce severe austenite grain growth. Upon rapid cooling, this region transforms into coarse, low-toughness martensite, becoming the primary site for Hydrogen-Induced Cold Cracking (HICC) .
Solidification (Hot) Cracking: Caused by low-melting FeS \text{FeS} FeS liquid films at dendrite boundaries under shrinkage stress. Prevented by maintaining Mn / S > 30 \text{Mn}/\text{S} > 30 Mn / S > 30 .
Hydrogen Cold Cracking Prevention: Requires preheating ( 150 – 250 ∘ C 150\text{--}250^{\circ}\text{C} 150 – 25 0 ∘ C ), low-hydrogen electrodes (AWS E7018), and post-weld heat treatment (PWHT).