Study guide
7.3 Placing, Finishing, Curing, and Testing (slump, cylinders)
NASCLA Contractor Study Guide Exam
Track your progress as you read
Finished sections get a check mark.
1 Coverage Map & Exam Overview
Coverage Map & Exam Overview
2 Business Organization, Licensing & Law
1.1 Business Entity Types and Formation 1.2 NASCLA Trade-Exam Waiver and Agency Licensing Boundaries 1.3 Construction Contract Law and Types of Contracts 1.4 Lien Law, Bond Claims, and Dispute Resolution
3 Financial Management, Tax & Labor Law
2.1 Financial Statements, Job Costing, and Cash Flow 2.2 Payroll, Federal/State Tax, and Recordkeeping 2.3 Labor & Employment Law (FLSA, immigration/I-9, EEO) 2.4 Insurance, Surety Bonds, and Risk Management
4 Estimating, Bidding & Plan Reading
3.1 Reading Construction Drawings and Specifications (CSI MasterFormat) 3.2 Quantity Takeoff and Material Estimating 3.3 Bidding, Markup, Overhead, and Profit 3.4 Change Orders, Allowances, and Unit Pricing
5 Project Management & Scheduling
4.1 Project Delivery Methods and the Submittal/RFI Process 4.2 Scheduling (CPM, Bar Charts, Critical Path) 4.3 Quality Control, Inspections, and Closeout 4.4 Permits, Codes, and the Inspection Process
6 Construction Safety & OSHA (29 CFR 1926)
5.1 OSHA Administration, Recordkeeping, and the General Duty Clause 5.2 Fall Protection, Scaffolds, and Ladders 5.3 Excavation/Trenching, Electrical, and Hazard Communication 5.4 PPE, Fire Protection, Cranes, and Confined Spaces
7 General Requirements & Sitework
6.1 Division 01 General Requirements and Temporary Facilities 6.2 Surveying, Site Layout, and Excavation 6.3 Soils, Compaction, and Erosion/Sediment Control 6.4 Foundations, Footings, and Site Drainage
8 Concrete (CSI Division 03)
7.1 Concrete Materials, Mix Design, and Water-Cement Ratio 7.2 Formwork and Reinforcement Placement 7.3 Placing, Finishing, Curing, and Testing (slump, cylinders) 7.4 Concrete Defects, Joints, and Cold-Weather Practices
9 Masonry (CSI Division 04)
8.1 Masonry Units, Mortar Types (M/S/N/O), and Grout 8.2 Brick and CMU Bonds, Reinforcement, and Coursing 8.3 Lintels, Control/Expansion Joints, and Flashing 8.4 Masonry Estimating and Cold/Hot Weather Construction
10 Metals & Wood (CSI Divisions 05 & 06)
9.1 Structural Steel, Connections, and Welding/Bolting 9.2 Light-Gauge Metal Framing 9.3 Wood Framing, Species/Grades, and Fasteners 9.4 Engineered Wood, Trusses, and Load Paths
11 Thermal & Moisture Protection (CSI Division 07)
10.1 Waterproofing, Dampproofing, and Below-Grade Protection 10.2 Insulation, R-Values, and Vapor Barriers 10.3 Roofing Systems (steep-slope and low-slope) and Underlayment 10.4 Flashing, Sealants, and Air Barriers
12 Openings & Finishes (CSI Divisions 08 & 09)
11.1 Doors, Windows, Glazing, and Hardware 11.2 Gypsum Board, Plaster, and Framing 11.3 Flooring, Tile, and Acoustical Ceilings 11.4 Painting, Coatings, and Finish Schedules
13 Mechanical, Plumbing & Electrical Overview
12.1 Plumbing Systems, Fixtures, and DWV/Supply Basics 12.2 HVAC Systems and Load Concepts 12.3 Electrical Systems, Service, and NEC Basics 12.4 Coordination, Rough-In, and Energy Code
7.3 Placing, Finishing, Curing, and Testing (slump, cylinders)
Key Takeaways Explain This Topic AI
Place concrete near final position; limit free-fall to ~4-5 ft and consolidate with vibration, but avoid over-vibration that causes segregation.
Slump (ASTM C143) measures workability; typical 1-4 in. High slump usually signals excess water and lower strength.
Never finish while bleed water is on the surface; trapped water causes scaling, dusting, and a weak crust.
Cure (ACI 308) at least 7 days; concrete reaches ~70% strength at 7 days and design f'c at 28 days, and lost hydration is not recoverable.
Test cylinders (ASTM C31/C39): strength = failure load / cross-sectional area; ACI acceptance is 3-test average >= f'c and no test more than 500 psi low.
Last updated: June 2026
Quality concrete depends as much on placing, finishing, curing, and testing as on mix design. This guide cross-references ACI 304 (placing), ASTM C143 (slump), ASTM C31 (field cylinders), and ASTM C39 (compressive testing). This editorial section practices field quality control, so use the test methods and acceptance criteria by reference.
Placing rules:
Deposit concrete as near its final position as possible; do not let it free-fall more than about 4-5 ft without a chute or tremie, or aggregate segregates .
Consolidate with internal vibrators to remove voids/honeycomb — but over-vibration causes segregation and bleeding (trap).
Do not place on frozen subgrade or in standing water.
Trap: dropping concrete from a great height into a deep wall form separates the coarse aggregate from the paste.
Slump (ASTM C143) measures consistency/workability using a 12-in cone filled in 3 layers, each rodded 25 times , then lifted; the slump is how far the concrete settles.
- Application Typical slump
- Pavement, footings 1-3 in
- Walls, slabs 2-4 in
- Columns, congested rebar 3-5 in
High slump usually means too much water -> low strength. Trap: a 6-in slump on a footing spec'd for 3 in signals an over-watered, weakened batch — reject it.
Finishing sequence (slabs):
Screeding/strikeoff — level to grade.
Bull floating/darbying — embed aggregate, level ridges. Do this before bleed water appears.
Wait for bleed water to evaporate — critical trap.
Floating — densify surface.
Troweling — hard, smooth finish (steel trowel).
Broom finish — texture for slip resistance (exterior walks/ramps).
Trap: finishing while bleed water is present traps it under the surface , causing scaling, dusting, and a weak crust.
Curing maintains moisture and temperature so cement can hydrate. Maintain moisture for at least 7 days for normal cement (ACI 308); concrete gains roughly 70% of design strength in 7 days and 100% (f'c) at 28 days .
Methods: water ponding/fogging, wet burlap, curing compounds (membrane), plastic sheeting. Trap: premature drying stops hydration and permanently lowers strength — strength is not recovered by re-wetting later.
Strength testing (ASTM C31/C39): Cast at least a set of cylinders per ACI (commonly one set per 150 CY or per 5,000 ft^2 of slab, per ACI 318). Standard cylinders are 6x12 in or 4x8 in , moist-cured, and broken in compression.
Worked numeric: A 6-in-diameter cylinder fails at 84,800 lb.
Area = pi x r^2 = 3.1416 x 3^2 = 28.27 in^2.
Strength = 84,800 / 28.27 = 3,000 psi .
Acceptance (ACI 318): the average of any 3 consecutive tests >= f'c , and no single test more than 500 psi below f'c .