Study guide

2.5 Plasma Arc Cutting (PAC): Torch Anatomy, Consumables, Gas Selection, Cut Quality & Safety

NCCER Boilermaker Exam

Track your progress as you read

Finished sections get a check mark.

1 Chapter 1: The Assessment, Boilermaker Craft, Safety, Tools & Crew Leadership

1.1 The NCCER Boilermaker Assessments: Format, Content Domains, Scoring & Credentials 1.2 Craft Fundamentals, Professional Roles & Industrial Safety 1.3 Confined Space Entry, Lockout/Tagout (LOTO) & Atmospheric Testing 1.4 Hand, Pneumatic, Electric & Hydraulic Boilermaker Tools 1.5 Crew Leadership, Job Planning, Production Tracking & Jobsite Communication

2 Chapter 2: Metallurgy, Base Materials, Oxyfuel, Air Carbon Arc & Plasma Cutting

2.1 Industrial Boiler Materials, Carbon & Alloy Steels, ASME Material Specs & Markings 2.2 Base Metal Surface Preparation, Joint Beveling & Fit-Up Cleanliness 2.3 Oxyfuel Cutting Principles, Equipment Setup, Torch Angles & Piercing Techniques 2.4 Air Carbon Arc Cutting and Gouging (CAC-A): Electrodes, Current, Air Supply, Technique & Defects 2.5 Plasma Arc Cutting (PAC): Torch Anatomy, Consumables, Gas Selection, Cut Quality & Safety

3 Chapter 3: Boiler Types, Steam Generation, Feedwater & Combustion Systems

3.1 Firetube Boiler Designs, Circulation Patterns & Operating Principles 3.2 Watertube Boiler Configurations, Natural & Forced Circulation, Drum Internals 3.3 Superheaters, Reheaters, Economizers & Air Heaters 3.4 Feedwater Systems, Deaerators, Condensate Return & Boiler Water Treatment 3.5 Combustion Systems: Burners, Stokers, Pulverizers, Fans & Draft Control

4 Chapter 4: Boiler Pressure & Nonpressure Components

4.1 Steam Drums, Mud Drums, Headers & Waterwalls 4.2 Nonpressure Components: Casing, Breeching, Baffles, Buckstays & Expansion Joints 4.3 Boiler Auxiliaries: Soot Blowers, Safety Valves, Gage Glasses & Blowdown Systems

5 Chapter 5: Valves, Gaskets, Fasteners, Anchors & Pipe Support Systems

5.1 Industrial Valve Types, Markings, Operation & Ratings 5.2 Gasket Materials, Flange Facings, Bolt Torque Sequences & Joint Assembly 5.3 Gasket Layout, Cutting & Fitting for Field-Made Gaskets 5.4 Fasteners, Anchors & Threaded Connection Hardware 5.5 Pipe Hangers, Supports, Rigid Restraints & Spring Can Installation/Adjustment

6 Chapter 6: Blueprint Reading, Welding Symbols & Construction Drawings

6.1 AWS Welding Symbols, Joint Geometry, Contours & NDE Designators 6.2 Piping Schematics, P&IDs, Isometric Drawings & Spool Sheets 6.3 Pressure Vessel General Arrangement, Detail Sheets, Coordinates & Elevations

7 Chapter 7: Trade Mathematics & Pipe Layout Calculations

7.1 Boilermaker Mechanical Trade Math: Offsets, Rolling Offsets & Travel Calculations 7.2 Vessel Volume, Surface Area, Circumference & Head Layout Computations 7.3 Mitered Turns, Segment Layout, Cutbacks & Branch Connections

8 Chapter 8: Pipe Fabrication - Socket Weld, Butt Weld, Threaded, Grooved & Spool Work

8.1 Pipe Materials, Nominal Pipe Size, Wall Schedules & Fitting Standards 8.2 Socket Weld Pipe Fabrication: The 1/16 in. Gap, Fillet Sizing & Cut Lengths 8.3 Butt Weld Pipe Fabrication: End Preparation, Alignment, Fit-Up & Cut Lengths 8.4 Pipe Layout Tools, Wrap-Arounds, Flange Squaring & Fabrication Tolerances 8.5 Threaded and Grooved Pipe Joining Systems 8.6 Spool Fabrication Workflow, Shop Versus Field Welds & Advanced Pipe Fabrication

9 Chapter 9: Tube Fabrication, Bending & Rolling

9.1 Boiler Tube Removal, Inspection, Wall Thinning & Replacement Criteria 9.2 Tube Preparation, Bending Radii, Ovality & Alignment Tolerances 9.3 Tube Expanding Mechanics, Rolling Torque Calculations, Wall Reduction & Flaring/Beading

10 Chapter 10: Welding Processes, Preheat & Stress Relieving

10.1 SMAW, GTAW & FCAW Welding Processes in Pressure Vessel Applications 10.2 Electrode Selection, Storage, Baking & AWS Filler Metal Classifications 10.3 Preheating Standards, Interpass Temperature Control & Post-Weld Heat Treatment (PWHT)

11 Chapter 11: Rigging Equipment, Hardware & Crane Operations

11.1 Rigging Hardware: Slings, Shackles, Eye Bolts & Inspection Criteria 11.2 Rigging Math: Sling Angles, Tension Calculations & Center of Gravity 11.3 Crane Signals, Load Charts, Boom Angle Deratings & Critical Lift Planning

12 Chapter 12: Towers, Heat Exchangers & Refractory/BRIL Systems

12.1 Shell-and-Tube Heat Exchangers: Bundles, Baffles & Floating Heads 12.2 Fractionation Towers, Trays, Downcomers, Packing & Vessel Hardware 12.3 Refractory Materials (Brick, Castable, Ceramic Fiber), Anchoring & Lagging (BRIL)

13 Chapter 13: ASME Codes, Quality Assurance, NDE, Pressure Testing & System Cleaning

13.1 ASME Boiler & Pressure Vessel Code (Sections I, VIII, IX) & NBIC Standards 13.2 Quality Control, Material Test Reports (MTRs), Weld Mapping & Traceability 13.3 Nondestructive Examination (NDE): VT, PT, MT, UT, RT & Discontinuity Evaluation 13.4 Hydrostatic and Pneumatic Testing Procedures, Safety Precautions & MAWP Validation 13.5 System Flushing, Chemical Cleaning, Boil-Out, Steam Blows & Service Leak Testing

2.5 Plasma Arc Cutting (PAC): Torch Anatomy, Consumables, Gas Selection, Cut Quality & Safety

Key Takeaways Explain This Topic AI

Plasma arc cutting severs stainless steel, aluminum, copper and nickel alloys that oxyfuel cannot cut, because it melts and blows metal out rather than burning it in oxygen.

The constricting nozzle orifice is the critical dimension; an oval or oversized orifice immediately produces bevelled, dross-heavy cuts.

Electrode and nozzle are replaced as a matched set, and the hafnium insert is condemned at the manufacturer's pit depth, commonly about 0.040 in.

Low-speed dross is heavy and chips off; high-speed dross is thin, hard and welded on — the two point to opposite corrections.

AWS Z49.1 plasma cutting shades scale with amperage, from minimum shade 4 below 20 A to minimum shade 10 at 400 to 800 A.

Last updated: August 2026

Plasma Arc Cutting (PAC): Torch Anatomy, Consumables, Cut Quality & Safety

Core Trade Concept: Oxyfuel cutting depends on the base metal burning in a stream of oxygen, which is why it stops working on stainless steel, aluminum, copper and nickel alloys — those metals form refractory oxides that will not sustain the reaction. Plasma Arc Cutting (PAC) does not care. It forces a gas through a constricting orifice and a high-current arc, ionizing the gas into a plasma jet at temperatures far above the melting point of any structural metal, then blows the melt out mechanically. For a boilermaker, PAC is the process that severs stainless tower internals, austenitic tube stubs, alloy trays and thin waterwall panel material where oxyfuel would fail or distort.

1. How the Process Works TRANSFERRED ARC PLASMA CUTTING

  • Power supply (-) ---> ELECTRODE (hafnium insert in copper)
  • |
  • [ swirl ring ] <-- imparts vortex to gas
  • |
  • [ NOZZLE ] <-- constricting orifice: the
  • | single most important
  • | dimension in the torch
  • ==== PLASMA JET ====
  • |
  • Power supply (+) ---> WORKPIECE (arc transfers to the work)

Constriction is the whole idea. Forcing the arc through a small nozzle orifice raises its current density and velocity enormously. A wider or wallowed-out orifice immediately degrades every quality parameter.

Transferred vs. non-transferred arc. In a transferred arc the work is part of the circuit and the arc jumps electrode-to-work; this is what all metal cutting uses. In a non-transferred arc the circuit is electrode-to-nozzle, used for spraying and for cutting non-conductive material. If a PAC torch will only pilot and will not transfer, suspect the work lead clamp.

Swirl. The swirl ring spins the gas so the hottest column stays centered. The vortex direction means one side of the kerf is always squarer than the other — on most torches, moving forward, the right-hand side is the good side . Lay out cuts so the scrap takes the bevelled side.

2. Torch Anatomy and Consumable Wear

Part Function Wear signature and limit

Electrode Emits the arc from a hafnium (or zirconium) insert pressed into copper The insert erodes into a pit . Replace at the pit depth in the manufacturer's manual — commonly about 0.040 in. (1 mm) . A blown-through electrode destroys the nozzle and can damage the torch head

Swirl ring Sets the gas vortex Cracks, blocked ports; replace with the electrode/nozzle set

Nozzle (tip) Constricts the arc Orifice goes oval or oversized ; gouged face. An out-of-round orifice produces a bevelled, dross-heavy cut

Shield cap / retaining cap Deflects molten spatter, sets standoff Spatter build-up, damaged threads

Replace the electrode and nozzle as a matched set. Running a new nozzle on a worn electrode simply destroys the new nozzle. The classic field mistake is to change only the part that looks worst.

Air quality is a consumable issue. Plasma air must be clean, dry and oil-free . Moisture and compressor oil are the leading cause of short consumable life, double arcing (an arc that jumps electrode-to-nozzle-to-work and burns the nozzle out), and dirty cut faces.

3. Gas Selection

  • Plasma gas Typical use
  • Compressed air The general-purpose choice for carbon steel, stainless and aluminum on portable field units
  • Oxygen Best cut quality and speed on carbon steel; shortens electrode life on non-ferrous
  • Nitrogen Stainless steel and aluminum; clean cut face, good electrode life
  • Argon–hydrogen (H35) Heavy stainless and aluminum sections; highest heat content

For boilermaker field work, compressed air covers most cutting; nitrogen or argon–hydrogen appear on shop tables cutting thick stainless internals.

4. Cut Quality: Speed, Standoff and Dross

Three variables control the cut, and two of the three failures look similar until you learn the difference. TRAVEL SPEED TOO SLOW CORRECT SPEED TOO FAST

  • +-------------------+ +-----------------+ +-----------------+
  • | Wide kerf | | Narrow kerf | | Narrow kerf |
  • | LOW-SPEED DROSS: | | Little/no dross | | HIGH-SPEED |
  • | heavy, bubbly | | Arc lag 5-10 deg| | DROSS: thin, |
  • | slag, chips off | | | | hard, welded on |
  • | Excess heat/taper | | | | Cut may not sever|
  • +-------------------+ +-----------------+ +-----------------+

Low-speed dross forms a heavy, bubbly bead on the underside that usually chips off with a scraper. It signals travel too slow, amperage too high, or standoff too small.

High-speed dross is a thin, hard, tightly adherent bead that must be ground. It signals travel too fast, amperage too low, or standoff too great — and is frequently accompanied by an incomplete cut and a trailing arc lag greater than about 10°.

Standoff (nozzle-to-work distance) is set by the manufacturer's chart and held constant with a drag shield or a stand-off guide. Increasing standoff widens the kerf, increases bevel and shortens consumable life.

Piercing. Never pierce with the nozzle sitting on the plate. Start at an angle so the initial blowback is directed away from the torch, then rotate upright. Rated pierce thickness is typically about half the rated severance thickness for a given machine — a unit that severs 1 in. will usually only pierce 1/2 in. reliably.

5. PAC Compared With Oxyfuel and CAC-A

  • Oxyfuel (OFC) Plasma (PAC) Air carbon arc (CAC-A)
  • Cuts stainless / aluminum / copper No (without powder injection) Yes Yes (removes metal)
  • Heat-affected zone Widest Narrow Moderate
  • Distortion on thin material High Low Moderate
  • Best economics on very thick carbon steel Yes No No

Primary boilermaker use Plate, structural, heavy severance Stainless internals, tube stubs, thin panel Back-gouging, defect excavation

  • Electrical shock hazard None from the torch Yes — open-circuit voltage Yes
  • 6. Safety

Electric shock is the differentiating hazard. PAC power supplies run high open-circuit DC voltage and the torch carries it. Never change consumables with the machine energised; never operate with a damaged torch lead; never bypass the torch safety interlock that prevents firing with the retaining cap loose.

Eye protection scales with amperage. From AWS Z49.1 Table 1, plasma arc cutting minimum protective shades are: less than 20 A — shade 4; 20–40 A — 5; 40–60 A — 6; 60–80 A — 8; 80–300 A — 8 (suggested 9); 300–400 A — 9 (suggested 12); 400–800 A — 10 (suggested 14) . Do not carry the shade 12–14 habit from gouging down to a 45 A portable unit, and do not carry a shade 5 habit up to a 400 A table.

Fume. Cutting stainless and other chromium-bearing alloys generates hexavalent chromium . Local exhaust or a water table is required, and inside a vessel this becomes a respiratory protection question, not a ventilation preference.

Noise. A plasma jet is a supersonic gas jet; hearing protection is mandatory.

Fire. Sparks from arc cutting travel in excess of 35 ft. Hot work permit, fire watch, and coverage of everything below the cut.

Compressed gas. Air lines at 90–120 psi whip when they part; use whip checks and safety pins on couplings exactly as for pneumatic tools.

7. Realistic Trade Scenario: Removing 304 Stainless Tray Rings From a Fractionation Tower

A turnaround crew must remove twelve corroded Type 304 stainless tray support rings, seal-welded to the inside wall of a carbon steel column, without gouging the shell.

Oxyfuel is ruled out — 304 stainless forms chromium oxide with a melting point far above the base metal, so the cut will not sustain itself.

CAC-A is ruled out for this cut — it would remove metal aggressively and risks carbon and copper contamination on the shell wall that must later be re-welded.

PAC on compressed air is selected: narrow kerf, minimal heat input, controllable depth. The crew sets standoff with a drag shield, plans each cut so the square side of the kerf falls on the shell side, and stops the cut short of the shell, finishing the last 1/16 in. with a grinder so the pressure boundary is never arced.

Confined space controls dominate the plan : hexavalent chromium fume from the 304, forced local exhaust at the cut, continuous atmospheric monitoring, and an attendant at the manway. The electrical hazard of the torch inside a wet, conductive steel vessel drives the use of a GFCI-protected supply and a rigorous consumable-change lockout.