Study guide
9.2 Tube Preparation, Bending Radii, Ovality & Alignment Tolerances
NCCER Boilermaker Exam
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: The Assessment, Boilermaker Craft, Safety, Tools & Crew Leadership
1.1 The NCCER Boilermaker Assessments: Format, Content Domains, Scoring & Credentials 1.2 Craft Fundamentals, Professional Roles & Industrial Safety 1.3 Confined Space Entry, Lockout/Tagout (LOTO) & Atmospheric Testing 1.4 Hand, Pneumatic, Electric & Hydraulic Boilermaker Tools 1.5 Crew Leadership, Job Planning, Production Tracking & Jobsite Communication
2 Chapter 2: Metallurgy, Base Materials, Oxyfuel, Air Carbon Arc & Plasma Cutting
2.1 Industrial Boiler Materials, Carbon & Alloy Steels, ASME Material Specs & Markings 2.2 Base Metal Surface Preparation, Joint Beveling & Fit-Up Cleanliness 2.3 Oxyfuel Cutting Principles, Equipment Setup, Torch Angles & Piercing Techniques 2.4 Air Carbon Arc Cutting and Gouging (CAC-A): Electrodes, Current, Air Supply, Technique & Defects 2.5 Plasma Arc Cutting (PAC): Torch Anatomy, Consumables, Gas Selection, Cut Quality & Safety
3 Chapter 3: Boiler Types, Steam Generation, Feedwater & Combustion Systems
3.1 Firetube Boiler Designs, Circulation Patterns & Operating Principles 3.2 Watertube Boiler Configurations, Natural & Forced Circulation, Drum Internals 3.3 Superheaters, Reheaters, Economizers & Air Heaters 3.4 Feedwater Systems, Deaerators, Condensate Return & Boiler Water Treatment 3.5 Combustion Systems: Burners, Stokers, Pulverizers, Fans & Draft Control
4 Chapter 4: Boiler Pressure & Nonpressure Components
4.1 Steam Drums, Mud Drums, Headers & Waterwalls 4.2 Nonpressure Components: Casing, Breeching, Baffles, Buckstays & Expansion Joints 4.3 Boiler Auxiliaries: Soot Blowers, Safety Valves, Gage Glasses & Blowdown Systems
5 Chapter 5: Valves, Gaskets, Fasteners, Anchors & Pipe Support Systems
5.1 Industrial Valve Types, Markings, Operation & Ratings 5.2 Gasket Materials, Flange Facings, Bolt Torque Sequences & Joint Assembly 5.3 Gasket Layout, Cutting & Fitting for Field-Made Gaskets 5.4 Fasteners, Anchors & Threaded Connection Hardware 5.5 Pipe Hangers, Supports, Rigid Restraints & Spring Can Installation/Adjustment
6 Chapter 6: Blueprint Reading, Welding Symbols & Construction Drawings
6.1 AWS Welding Symbols, Joint Geometry, Contours & NDE Designators 6.2 Piping Schematics, P&IDs, Isometric Drawings & Spool Sheets 6.3 Pressure Vessel General Arrangement, Detail Sheets, Coordinates & Elevations
7 Chapter 7: Trade Mathematics & Pipe Layout Calculations
7.1 Boilermaker Mechanical Trade Math: Offsets, Rolling Offsets & Travel Calculations 7.2 Vessel Volume, Surface Area, Circumference & Head Layout Computations 7.3 Mitered Turns, Segment Layout, Cutbacks & Branch Connections
8 Chapter 8: Pipe Fabrication - Socket Weld, Butt Weld, Threaded, Grooved & Spool Work
8.1 Pipe Materials, Nominal Pipe Size, Wall Schedules & Fitting Standards 8.2 Socket Weld Pipe Fabrication: The 1/16 in. Gap, Fillet Sizing & Cut Lengths 8.3 Butt Weld Pipe Fabrication: End Preparation, Alignment, Fit-Up & Cut Lengths 8.4 Pipe Layout Tools, Wrap-Arounds, Flange Squaring & Fabrication Tolerances 8.5 Threaded and Grooved Pipe Joining Systems 8.6 Spool Fabrication Workflow, Shop Versus Field Welds & Advanced Pipe Fabrication
9 Chapter 9: Tube Fabrication, Bending & Rolling
9.1 Boiler Tube Removal, Inspection, Wall Thinning & Replacement Criteria 9.2 Tube Preparation, Bending Radii, Ovality & Alignment Tolerances 9.3 Tube Expanding Mechanics, Rolling Torque Calculations, Wall Reduction & Flaring/Beading
10 Chapter 10: Welding Processes, Preheat & Stress Relieving
10.1 SMAW, GTAW & FCAW Welding Processes in Pressure Vessel Applications 10.2 Electrode Selection, Storage, Baking & AWS Filler Metal Classifications 10.3 Preheating Standards, Interpass Temperature Control & Post-Weld Heat Treatment (PWHT)
11 Chapter 11: Rigging Equipment, Hardware & Crane Operations
11.1 Rigging Hardware: Slings, Shackles, Eye Bolts & Inspection Criteria 11.2 Rigging Math: Sling Angles, Tension Calculations & Center of Gravity 11.3 Crane Signals, Load Charts, Boom Angle Deratings & Critical Lift Planning
12 Chapter 12: Towers, Heat Exchangers & Refractory/BRIL Systems
12.1 Shell-and-Tube Heat Exchangers: Bundles, Baffles & Floating Heads 12.2 Fractionation Towers, Trays, Downcomers, Packing & Vessel Hardware 12.3 Refractory Materials (Brick, Castable, Ceramic Fiber), Anchoring & Lagging (BRIL)
13 Chapter 13: ASME Codes, Quality Assurance, NDE, Pressure Testing & System Cleaning
13.1 ASME Boiler & Pressure Vessel Code (Sections I, VIII, IX) & NBIC Standards 13.2 Quality Control, Material Test Reports (MTRs), Weld Mapping & Traceability 13.3 Nondestructive Examination (NDE): VT, PT, MT, UT, RT & Discontinuity Evaluation 13.4 Hydrostatic and Pneumatic Testing Procedures, Safety Precautions & MAWP Validation 13.5 System Flushing, Chemical Cleaning, Boil-Out, Steam Blows & Service Leak Testing
9.2 Tube Preparation, Bending Radii, Ovality & Alignment Tolerances
Key Takeaways Explain This Topic AI
Boiler tube alloys span SA-178 (electric resistance welded carbon steel), SA-192 (seamless high-pressure carbon steel), SA-210 (medium-carbon high-strength steel), and SA-213 (ferritic/austenitic chrome-moly alloys including T11, T22, and T91).
Mandrel rotary draw bending utilizes bend dies, clamp dies, pressure dies, wiper dies, and internal ball/bullet mandrels to prevent extrados flattening and intrados wrinkling on tight-radius bends.
The minimum cold bend radius is generally R m i n ≥ 2.5 × O D R_{min} \ge 2.5 \times OD R min ≥ 2.5 × O D ; bending produces wall thinning on the tensile outer radius (extrados) and thickening on the compressive inner radius (intrados).
ASME Section I and NBIC mandate that tube ovality (out-of-roundness) must not exceed 8%–10%, calculated as % Ovality = ((D_max - D_min) / D_nom) * 100%.
Tube end preparation requires de-burring, chamfering, and polishing both the internal and external surfaces to bare bright metal for a minimum of 2 to 3 inches from each end.
Last updated: August 2026
8.2 Tube Preparation, Bending Radii, Ovality & Alignment Tolerances
Core Trade Concept: Fabricating and bending replacement boiler tubes requires strict compliance with ASME Section I material specifications, geometric bending limits, and surface preparation standards. Bending alters tube wall geometry—stretching and thinning the outer radius ( extrados ) while compressing and thickening the inner radius ( intrados ). Boilermakers must calculate wall thinning, measure ovality, enforce post-bend heat treatment rules, and prepare tube ends to pristine bare metal.
1. Boiler Tube Material Specifications & Metallurgy
Boiler tubes are classified by manufacturing method (seamless vs. welded), carbon content, and alloying elements. Selecting the correct ASME Section II / Section I material specification is vital for pressure integrity, corrosion resistance, and high-temperature creep strength. BOILER TUBE METALLURGY SPECTRUM
LOW TEMPERATURE / LOW-MEDIUM PRESSURE =====> HIGH TEMPERATURE / HIGH PRESSURE
- +---------------+ +---------------+ +---------------+ +---------------+
- | SA-178 | | SA-192 | | SA-210 | | SA-213 |
- | (ERW Carbon) | | (Seamless CS) | | (Med-Carbon) | | (Chrome-Moly) |
- +---------------+ +---------------+ +---------------+ +---------------+
- Grade A: Low C - Seamless drawn - Grade A-1 / C - T11 (1.25Cr-0.5Mo)
- Grade C: Med C - High-pressure - 60-70 ksi TS - T22 (2.25Cr-1Mo)
- Firetubes & - Generating banks - High-heat-flux - T91 (9Cr-1Mo-V)
- Waterwalls - Superheaters Waterwalls - TP304H/347H SS
- Material Classifications
ASME SA-178 (Electric Resistance Welded Carbon Steel):
Description: Manufactured from flat steel strip formed into a cylinder and joined by high-frequency resistance welding without filler metal. Grade A is low-carbon ( 0.06 – 0.18 % C 0.06\text{--}0.18\%\text{ C} 0.06 – 0.18% C ); Grade C is medium-carbon ( 0.35 % C 0.35\%\text{ C} 0.35% C max, tensile strength ≥ 60 ksi \ge 60\text{ ksi} ≥ 60 ksi ).
Applications: Firetube boilers, low-to-medium pressure watertube generating banks, and waterwall panels operating below 800 ∘ F 800^\circ\text{F} 80 0 ∘ F .
ASME SA-192 (Seamless Carbon Steel for High-Pressure Service):
Description: Hot-finished or cold-drawn seamless carbon steel ( 0.06 – 0.18 % C 0.06\text{--}0.18\%\text{ C} 0.06 – 0.18% C ) engineered for severe high-pressure service.
Applications: Utility and industrial steam drums, economizers, and generating banks operating up to 850 ∘ F 850^\circ\text{F} 85 0 ∘ F .
ASME SA-210 (Seamless Medium-Carbon Steel):
Description: Higher-strength carbon steel tubing (Grade A-1: 60 ksi 60\text{ ksi} 60 ksi tensile; Grade C: 70 ksi 70\text{ ksi} 70 ksi tensile). Higher carbon content provides higher allowable stress values, allowing thinner tube walls.
Applications: High-heat-flux furnace waterwall panels and riser circuits.
ASME SA-213 (Seamless Ferritic and Austenitic Alloy Steel):
Description: High-temperature, creep-resistant alloy tubing formulated with chromium (for oxidation/corrosion resistance), molybdenum (for creep strength), and vanadium/nitrogen (for carbide stabilization).
Grade T11 ( 1.25 % Cr – 0.5 % Mo 1.25\%\text{ Cr -- }0.5\%\text{ Mo} 1.25% Cr – 0.5% Mo ): Economizer and low-temperature superheater passes up to 950 ∘ F 950^\circ\text{F} 95 0 ∘ F .
Grade T22 ( 2.25 % Cr – 1.0 % Mo 2.25\%\text{ Cr -- }1.0\%\text{ Mo} 2.25% Cr – 1.0% Mo ): High-temperature superheaters and reheaters up to 1,050 ∘ F 1{,}050^\circ\text{F} 1 , 05 0 ∘ F .
Grade T91 ( 9 % Cr – 1 % Mo – V 9\%\text{ Cr -- }1\%\text{ Mo -- V} 9% Cr – 1% Mo – V ): Advanced martensitic alloy engineered for supercritical and ultra-supercritical superheater/reheater circuits up to 1,150 ∘ F 1{,}150^\circ\text{F} 1 , 15 0 ∘ F . Requires strict preheat, interpass, and controlled post-weld/post-bend heat treatments.
Grades TP304H / TP347H (Austenitic Stainless Steels): High-temperature superheater/reheater finishing loops operating above 1,100 ∘ F 1{,}100^\circ\text{F} 1 , 10 0 ∘ F under severe coal/biomass ash corrosion conditions.
2. Tube Bending Mechanics & Tooling: Rotary Draw vs. Ram Bending
Boiler tubes must be bent to precise angles and radii to route around burner throats, sootblower wallboxes, inspection doors, and drum penetrations. MANDREL ROTARY DRAW BENDER TOOLING
- [ Clamp Die ]
- |
- v
- +-----------------------+=======+ (Tube Clamped Rigidly to Bend Die)
- | Wiper Die | TUBE |
- +-----------------------+=======+--------+
- | Pressure Die ===> | | Bend |
- +-----------------------+ | Die |
- ^ | (Rotates
- | | with |
- [ Internal Mandrel ] | Tube) |
- (Bullet or Ball Mandrel +--------+
- positioned inside tube at tangency point)
- Tooling Components of Rotary Draw Benders
Mandrel rotary draw bending is the premier industrial process for fabricating high-precision, wrinkle-free boiler tube bends:
Bend Die (Radius Die): A circular die machined with a matching tube contour groove that rotates to pull the tube around the specified centerline bend radius ( C L R CLR C L R ).
Clamp Die: Clamps the leading straight section of the tube securely against the bend die, rotating synchronously with it.
Pressure Die: Supports the outer tube wall along the straight trailing section, feeding forward to prevent the tube from kicking outward while absorbing reaction forces.
Wiper Die: Positioned immediately behind the bend die tangency point on the inner radius (intrados). It prevents the compressive forces on the inside curve from buckling into structural ripples or wrinkles .
Internal Mandrel: A precision tool steel or aluminum-bronze mandrel (bullet plug or multi-ball flexible linkage) inserted inside the tube bore directly at the tangency point. The mandrel supports the tube from within, preventing the tensile outer wall from collapsing inward or flattening.
Rotary Draw Bending vs. Ram (Press) Bending
Feature / Parameter Mandrel Rotary Draw Bending Ram (Press) Bending
Mechanism Tube is clamped and drawn around a rotating bend die with internal mandrel support. A central ram die pushes the tube between two pivoting stationary wing counter-dies.
Internal Support Internal bullet or flexible ball mandrel prevents cross-sectional collapse. No internal mandrel support.
Bend Radius Capability Tight radii: 1.5 × OD to 3.0 × OD 1.5\times\text{OD to }3.0\times\text{OD} 1.5 × OD to 3.0 × OD with minimal ovality. Large sweeping radii only: > 4.0 × to 5.0 × OD > 4.0\times\text{ to }5.0\times\text{OD} > 4.0 × to 5.0 × OD .
Wall Thinning & Ovality Highly controlled; ovality typically < 3 % – 5 % < 3\%\text{--}5\% < 3% – 5% . Severe cross-sectional flattening; ovality often exceeds 10 % – 15 % 10\%\text{--}15\% 10% – 15% .
Code Suitability Standard for ASME Section I utility superheater/generating tubes. Restricted to field structural bends or non-critical piping; unacceptable for tight boiler bends.
Cold Bending vs. Hot Bending
Cold Bending: Performed at ambient temperatures below the lower transformation temperature ( < 1,300 ∘ F < 1{,}300^\circ\text{F} < 1 , 30 0 ∘ F ). Highly efficient, accurate, and preserves clean surface finish. Produces strain hardening (cold work) in the extrados, which may require post-bend heat treatment depending on material alloy and bend severity.
Hot Bending: Performed by heating the tube bend zone to forging temperatures ( 1,600 ∘ F– 1,950 ∘ F 1{,}600^\circ\text{F}\text{--}1{,}950^\circ\text{F} 1 , 60 0 ∘ F – 1 , 95 0 ∘ F ) using induction coils or gas furnaces. Used for heavy-wall tubing or ultra-tight bends ( < 1.5 × O D < 1.5 \times OD < 1.5 × O D ).
Precautions: Hot bending must be performed under strict pyrometric temperature monitoring. Overheating ( > 2,000 ∘ F > 2{,}000^\circ\text{F} > 2 , 00 0 ∘ F ) causes rapid grain growth, severe decarburization, and heavy internal/external scaling.
3. Minimum Bend Radii, Wall Thinning & Thickening Calculations
During bending, the metal along the outer radius ( extrados ) experiences severe tensile stretching, causing wall thinning. Simultaneously, metal along the inner radius ( intrados ) experiences compressive forces, causing wall thickening and risk of wrinkling. BEND GEOMETRY & WALL THICKNESS DYNAMICS
- EXTRADOS (Outer Radius)
- Tensile Stretch ===> Wall Thinning
- /-------------------\
- / t_extrados \
- / (Thinned Wall) \
- | |
- Straight Leg | Centerline | Straight Leg
- ============================| Radius (CLR) |============================
- (Nominal Wall t_orig) | | (Nominal Wall t_orig)
- \ /
- \ t_intrados /
- \-------------------/
- INTRADOS (Inner Radius)
- Compressive Strain ===> Wall Thickening
- Minimum Bend Radius ( R m i n R_{min} R min )
Under standard boiler manufacturing practices and ASME Section I (PG-19) :
The recommended minimum centerline bend radius ( C L R CLR C L R or R R R ) for cold-formed boiler tubes is R ≥ 2.5 × O D R \ge 2.5 \times OD R ≥ 2.5 × O D (or 3.0 × O D 3.0 \times OD 3.0 × O D for seamless alloy tubes without special mandrel tooling).
Ultra-tight bends ( R < 2.0 × O D R < 2.0 \times OD R < 2.0 × O D ) require heavy-wall starting stock or hot induction forming to ensure the thinned extrados maintains structural integrity.
Wall Thinning Calculation Formulas
The theoretical wall thickness at the extrados ( t e x t r a d o s t_{extrados} t e x t r a d os ) after bending is approximated by: t e x t r a d o s ≈ t o r i g ⋅ ( R R + 0.5 ⋅ O D ) t_{extrados} \approx t_{orig} \cdot \left( \frac{R}{R + 0.5 \cdot OD} \right) t e x t r a d os ≈ t or i g ⋅ ( R + 0.5 ⋅ O D R )
Where:
- t o r i g = t_{orig} = t or i g = Original nominal tube wall thickness before bending (inches)
- R = R = R = Centerline bend radius ( C L R CLR C L R , inches)
- O D = OD = O D = Nominal outside diameter of the tube (inches)
The Percentage Wall Thinning is calculated using the measured thinned wall ( t m i n t_{min} t min ): % Wall Thinning = ( t o r i g − t m i n t o r i g ) × 100 % \%\text{ Wall Thinning} = \left( \frac{t_{orig} - t_{min}}{t_{orig}} \right) \times 100\% % Wall Thinning = ( t or i g t or i g − t min ) × 100%
Worked Example: \text{Worked Example:} Worked Example: A boilermaker cold-bends a 2.500 -inch OD 2.500\text{-inch OD} 2.500 -inch OD SA-210 Grade A1 boiler tube with original wall thickness t o r i g = 0.220 inches t_{orig} = 0.220\text{ inches} t or i g = 0.220 inches to a centerline radius R = 6.250 inches R = 6.250\text{ inches} R = 6.250 inches ( 2.5 × O D 2.5 \times OD 2.5 × O D ): t e x t r a d o s ≈ 0.220 ⋅ ( 6.250 6.250 + ( 0.5 ⋅ 2.500 ) ) = 0.220 ⋅ ( 6.250 7.500 ) = 0.220 ⋅ 0.8333 = 0.1833 inches t_{extrados} \approx 0.220 \cdot \left( \frac{6.250}{6.250 + (0.5 \cdot 2.500)} \right) = 0.220 \cdot \left( \frac{6.250}{7.500} \right) = 0.220 \cdot 0.8333 = 0.1833\text{ inches} t e x t r a d os ≈ 0.220 ⋅ ( 6.250 + ( 0.5 ⋅ 2.500 ) 6.250 ) = 0.220 ⋅ ( 7.500 6.250 ) = 0.220 ⋅ 0.8333 = 0.1833 inches % Wall Thinning = ( 0.220 − 0.1833 0.220 ) × 100 % = ( 0.0367 0.220 ) × 100 % = 16.68 % \%\text{ Wall Thinning} = \left( \frac{0.220 - 0.1833}{0.220} \right) \times 100\% = \left( \frac{0.0367}{0.220} \right) \times 100\% = 16.68\% % Wall Thinning = ( 0.220 0.220 − 0.1833 ) × 100% = ( 0.220 0.0367 ) × 100% = 16.68%
Critical ASME Code Rule: The resulting thinned wall thickness at the extrados ( t e x t r a d o s t_{extrados} t e x t r a d os ) must never fall below the ASME Section I PG-27 minimum design wall thickness ( t m i n t_{min} t min ) for the boiler's design pressure and temperature. If calculations show t e x t r a d o s < t m i n t_{extrados} < t_{min} t e x t r a d os < t min , the fabricator must select heavier-wall starting stock.
- 4. Ovality (Out-of-Roundness) Standards & Post-Bend Heat Treatment
- Ovality Calculation & Tolerances
When a tube is bent, the tensile and compressive forces naturally tend to collapse the circular cross-section into an ellipse. Ovality (out-of-roundness) restricts internal steam/water flow and increases pressure drop. TUBE OVALITY CROSS-SECTION
- D_max (Major Axis / Vertical)
- ^
- |
- +-----+-----+
- / \
- D_min <==== | | ====> D_min
- (Minor Axis) \ / (Minor Axis)
- +-----+-----+
- |
- v
- D_max (Major Axis / Vertical)
Under ASME Section I (PG-19.1) and industry standards, ovality is calculated as: % Ovality = ( D m a x − D m i n D n o m ) × 100 % \%\text{ Ovality} = \left( \frac{D_{max} - D_{min}}{D_{nom}} \right) \times 100\% % Ovality = ( D n o m D ma x − D min ) × 100%
Where:
D m a x = D_{max} = D ma x = Maximum measured outside diameter across the flattened bend (inches)
D m i n = D_{min} = D min = Minimum measured outside diameter across the flattened bend (inches)
D n o m = D_{nom} = D n o m = Original nominal tube outside diameter (inches)
ASME / NBIC Acceptance Limit: Ovality must not exceed 8 % to 10 % 8\%\text{ to }10\% 8% to 10% for general boiler tubes. In high-pressure superheaters or tight-pitch waterwalls, specifications frequently tighten this limit to ≤ 5 % \le 5\% ≤ 5% .
Post-Bend Heat Treatment (PBHT) Requirements
Cold bending induces severe plastic deformation, generating high residual tensile stresses and strain hardening that reduce material toughness and accelerate stress-corrosion cracking or creep embrittlement.
Under ASME Section I (Table PW-10 / PG-19) , post-forming heat treatment is mandatory for cold-formed alloy tubes when the calculated outer fiber elongation (strain) exceeds specific thresholds: Outer Fiber Strain ( % ) = ( O D 2 R ) × 100 % \text{Outer Fiber Strain } (\%) = \left( \frac{OD}{2R} \right) \times 100\% Outer Fiber Strain ( % ) = ( 2 R O D ) × 100%
Tube Material Specification Outer Fiber Strain Threshold Requiring PBHT Mandatory Heat Treatment Procedure
Carbon Steels (SA-178, SA-192, SA-210) > 12 % – 14 % > 12\%\text{--}14\% > 12% – 14% strain Stress relief at 1,100 ∘ F– 1,200 ∘ F 1{,}100^\circ\text{F}\text{--}1{,}200^\circ\text{F} 1 , 10 0 ∘ F – 1 , 20 0 ∘ F if design temp > 750 ∘ F > 750^\circ\text{F} > 75 0 ∘ F or in severe sour/corrosive service.
Low-Alloy Steels (SA-213 T11, T22) > 5 % strain > 5\%\text{ strain} > 5% strain (or R < 10 × O D R < 10 \times OD R < 10 × O D ) Subcritical stress relief / temper at 1,250 ∘ F– 1,350 ∘ F 1{,}250^\circ\text{F}\text{--}1{,}350^\circ\text{F} 1 , 25 0 ∘ F – 1 , 35 0 ∘ F for 1 hour per inch of thickness.
Martensitic Alloy (SA-213 T91) All cold bends exceeding 5 % 5\% 5% strain Full furnace Normalizing ( 1,900 ∘ F– 1,975 ∘ F 1{,}900^\circ\text{F}\text{--}1{,}975^\circ\text{F} 1 , 90 0 ∘ F – 1 , 97 5 ∘ F ) followed by Tempering ( 1,350 ∘ F– 1,425 ∘ F 1{,}350^\circ\text{F}\text{--}1{,}425^\circ\text{F} 1 , 35 0 ∘ F – 1 , 42 5 ∘ F ) . Subcritical stress relief alone is prohibited for T91 cold bends.
Austenitic Stainless (TP304H, TP347H) > 15 % strain > 15\%\text{ strain} > 15% strain Full Solution Anneal at 2,050 ∘ F– 2,150 ∘ F 2{,}050^\circ\text{F}\text{--}2{,}150^\circ\text{F} 2 , 05 0 ∘ F – 2 , 15 0 ∘ F followed by rapid water quench.
5. Tube End Preparation & Fit-up Standards
Before replacement tubes are installed into drums, headers, or waterwall panels, the tube ends must undergo meticulous mechanical preparation. TUBE END PREPARATION SPECIFICATION
- Bare Bright Metal Polished Zone (Internal & External)
- |<====== 2" to 3" ======>|
- +==============+------------------------+
- | Tube Wall | Ground 37.5° Bevel |
- | | Chamfered ID / Deburred| ===> 1/16" Root Face (Land)
- +==============+------------------------+
- | Tube Bore |
- +==============+------------------------+
- | Tube Wall | |
- +==============+------------------------+
Sizing & Gauge Ball Check: Tube ends must be sized to ensure circularity within ± 0.010 in. \pm 0.010\text{ in.} ± 0.010 in. of nominal ID/OD. Fabricators pass a hardened steel gauge ball (sized to 95 % 95\% 95% of nominal ID) through the entire length of bent tubes to verify there are no internal obstructions, excessive ovality, or unobserved kinks.
De-Burring & Chamfering: All sharp internal and external edges resulting from saw or abrasive wheel cutting must be fully deburred using rotary chamfering tools or fine files. Removing internal sharp burrs prevents damage to roller expanders and eliminates stress concentration risers.
Bare Bright Metal Cleaning:
The internal and external surfaces of each tube end must be cleaned to bare bright metal for a minimum distance of 2 to 3 inches 2\text{ to }3\text{ inches} 2 to 3 inches ( 50 to 75 mm 50\text{ to }75\text{ mm} 50 to 75 mm ) from the end.
Contaminant Removal: Boilermakers use pneumatic flap wheels, non-chlorinated solvent wipes, or silicon-carbide emery cloth to remove all mill scale, rust, varnish, paint, grease, and anti-spatter oils. Any residual varnish or oil will cause porosity in seal welds or compromise friction holding power in rolled joints.