Study guide

16.2 Corrosion Mechanisms, Materials Degradation, and Prevention

PE Chemical Exam

Track your progress as you read

Finished sections get a check mark.

1 Introduction & Exam Overview

About the PE Chemical Exam How to Use This Guide and the NCEES Handbook

2 Chapter 1: Material Balances & Flowsheet Calculations

1.1 Degree-of-Freedom Analysis & Process Flowsheet Accounting 1.2 Steady-State Material Balances (Reactive & Non-Reactive Systems) 1.3 Recycle, Bypass, and Purge Operations

3 Chapter 2: Energy Balances & Thermochemistry

2.1 Enthalpy Accounting, Sensible Heat, and Phase Changes 2.2 Heats of Reaction, Formation, and Adiabatic Flame Temperatures 2.3 Unsteady-State Mass and Energy Balances

4 Chapter 3: Fluid Statics & Incompressible Pipe Flow

3.1 Fluid Statics, Pressure Measurement, and Manometry 3.2 Incompressible Flow, Friction Factors, and the Moody Diagram 3.3 Minor Losses, Equivalent Length, and Piping Networks 3.4 Pumps, Compressors, and NPSH Calculations

5 Chapter 4: Advanced Fluid Dynamics & Compressible Flow

4.1 Compressible Gas Flow, Sonic Velocity, and Choked Flow 4.2 Flow Measurement Devices (Orifices, Venturis, Rotameters) 4.3 Multiphase Flow and Fluidization Principles 4.4 Mixing, Agitation, and Agitator Scale-Up

6 Chapter 5: Thermodynamic Laws & Fundamental Relations

5.1 First and Second Laws, Heat Engines, and Carnot Efficiency 5.2 Entropy, Availability, and Exergy Analysis 5.3 Fundamental Property Relations and Maxwell Equations

7 Chapter 6: Real Gases & Equations of State

6.1 Volumetric Properties and Compressibility Factor Charts 6.2 Cubic Equations of State (vdW, RK, SRK, and Peng-Robinson) 6.3 Residual Properties and Enthalpy/Entropy Departure Functions

8 Chapter 7: Phase & Chemical Reaction Equilibria

7.1 Pure Component Vapor Pressure and Phase Equilibria 7.2 Vapor-Liquid Equilibrium (VLE), Raoult's Law, and Activity Coefficients 7.3 Chemical Reaction Equilibria and Equilibrium Constant Calculation

9 Chapter 8: Heat Transfer Mechanisms & Conduction

8.1 Steady-State Conduction in Planar, Cylindrical, and Spherical Geometries 8.2 Convective Heat Transfer and Dimensionless Correlations 8.3 Thermal Radiation, Emissivity, and Surface Radiation Exchange

10 Chapter 9: Heat Exchanger Design & Phase Change

9.1 Shell-and-Tube Exchanger Design, TEMA Standards, and LMTD 9.2 Effectiveness-NTU Method and Exchanger Rating 9.3 Boiling Regimes, Condensation Phenomena, and Fouling Resistances

11 Chapter 10: Mass Transfer Fundamentals & Diffusion

10.1 Molecular Diffusion, Fick's Laws, and Equimolar Counterdiffusion 10.2 Convective Mass Transfer and Film Theories 10.3 Mass Transfer Dimensionless Numbers (Sherwood, Schmidt, Peclet)

12 Chapter 11: Distillation Operations

11.1 Vapor-Liquid Equilibrium and Relative Volatility in Distillation 11.2 McCabe-Thiele Method for Binary Distillation 11.3 Packed vs Tray Columns, Flooding, and Tray Hydraulics 11.4 Multicomponent Distillation Fundamentals and Key Components

13 Chapter 12: Rate-Controlled & Equilibrium Separations

12.1 Gas Absorption, Stripping, and the Kremser Equation 12.2 Liquid-Liquid Extraction and Ternary Phase Equilibria 12.3 Adsorption, Membrane Separations, and Drying Operations 12.4 Filtration, Crystallization, and Solid-Fluid Separations

14 Chapter 13: Chemical Kinetics & Ideal Isothermal Reactors

13.1 Reaction Rates, Rate Laws, and Order of Reaction 13.2 Temperature Dependence and the Arrhenius Equation 13.3 Batch Reactors and Continuous Stirred-Tank Reactors (CSTR) 13.4 Plug Flow Reactors (PFR) and Reactor Combinations

15 Chapter 14: Non-Ideal Flow, Non-Isothermal Reactors & Catalysis

14.1 Yield, Selectivity, and Multiple Reactions (Series and Parallel) 14.2 Non-Isothermal Reactor Design and Thermal Runaway 14.3 Heterogeneous Catalysis, Thiele Modulus, and RTD Models

16 Chapter 15: Physical & Transport Properties of Fluids

15.1 Fluid Density, Specific Gravity, and Viscosity Correlations 15.2 Thermal Conductivity and Specific Heat Capacities 15.3 Estimation Methods and Corresponding States Principles

17 Chapter 16: Materials of Construction & Corrosion

16.1 Mechanical Properties and Materials Selection in Chemical Plants 16.2 Corrosion Mechanisms, Materials Degradation, and Prevention

18 Chapter 17: Process Safety & Pressure Relief Systems

17.1 Hazard Identification Methodologies (HAZOP, FMEA, What-If) 17.2 Pressure Relief Valve (PRV) and Rupture Disk Sizing 17.3 Flammability, Explosions, and Toxic Dispersion Limits 17.4 Inerting, Purging, Discharge Location, and Containment

19 Chapter 18: Process Control & Engineering Economics

18.1 Process Dynamics and Feedback Control Loops 18.2 PID Controller Tuning and Loop Stability 18.3 Chemical Plant Capital Cost Estimation and Profitability Analysis 18.4 Field Instrumentation, Control Valves, Alarms, and Safety Instrumented Systems

20 Chapter 19: Process Design, Equipment Selection & Environmental Compliance

19.1 Process Flow Diagrams, P&IDs, Scale-Up, and Plant Siting 19.2 Process Equipment Selection, Sizing, and Optimization 19.3 Emissions Evaluation, Mitigation, and Remediation

21 Chapter 20: Plant Operation, Reliability & Continuous Improvement

20.1 Operating Procedures, Startup, and Shutdown 20.2 Mechanical Integrity, Reliability, and Failure Mechanisms 20.3 Debottlenecking, Optimization, and Troubleshooting

16.2 Corrosion Mechanisms, Materials Degradation, and Prevention

Key Takeaways Explain This Topic AI

Aqueous corrosion is fundamentally electrochemical, coupling an anodic oxidation reaction ( M → M n + + n e − M \rightarrow M^{n+} + n e^- M → M n + + n e − ) with cathodic reduction reactions (hydrogen evolution or oxygen reduction); thermodynamics is governed by the Nernst equation E = E ∘ − ( R T / n F ) ln ⁡ Q E = E^\circ - (RT/nF) \ln Q E = E ∘ − ( RT / n F ) ln Q and mapped onto Pourbaix ( E -pH E\text{-pH} E -pH ) diagrams delineating immunity, active corrosion, and passivation.

Uniform corrosion penetration rate is calculated from mass loss via CPR = ( K Δ W ) / ( ρ A t ) \text{CPR} = (K \Delta W) / (\rho A t) CPR = ( K Δ W ) / ( ρ A t ) , where (K = 534) yields CPR \text{CPR} CPR in mils per year (mpy) when Δ W \Delta W Δ W is in mg, ρ \rho ρ in g/cm 3 \text{g/cm}^3 g/cm 3 , (A) in in 2 \text{in}^2 in 2 , and (t) in hours ( 1 mpy = 0.0254 mm/yr = 25.4 μ m/yr 1\text{ mpy} = 0.0254\text{ mm/yr} = 25.4\,\mu\text{m/yr} 1 mpy = 0.0254 mm/yr = 25.4 μ m/yr ); rates below 1 mpy are outstanding, 1-5 mpy excellent, and > 20 mpy >20\text{ mpy} > 20 mpy unacceptable.

Galvanic corrosion acceleration is dictated by the cathode-to-anode area ratio ( i A = i C [ A C / A A ] i_A = i_C [A_C / A_A] i A ​ = i C ​ [ A C ​ / A A ​ ] ); a large cathode coupled to a small anode produces disastrous localized penetration, whereas a small noble cathode on a large active anode is generally benign.

Resistance to localized pitting and crevice attack in chloride environments is quantified by the Pitting Resistance Equivalent Number ( PREN = % Cr + 3.3 % Mo + 16 % N \text{PREN} = \% \text{Cr} + 3.3\% \text{Mo} + 16\% \text{N} PREN = % Cr + 3.3% Mo + 16% N ); standard austenitic 304/316 grades ( PREN ≈ 19 − 25 \text{PREN} \approx 19-25 PREN ≈ 19 − 25 ) are vulnerable to pitting and chloride stress corrosion cracking (SCC) above 60 ∘ C 60^\circ\text{C} 6 0 ∘ C ( 140 ∘ F 140^\circ\text{F} 14 0 ∘ F ), whereas Duplex 2205 ( PREN ≈ 35 \text{PREN} \approx 35 PREN ≈ 35 ) and Super Duplex 2507 ( PREN ≥ 40 \text{PREN} \ge 40 PREN ≥ 40 ) provide robust protection.

High-Temperature Hydrogen Attack (HTHA) occurs when atomic hydrogen reacts with iron carbides in steel ( Fe 3 C + 4 H → 3 Fe + CH 4 \text{Fe}_3\text{C} + 4\text{H} \rightarrow 3\text{Fe} + \text{CH}_4 Fe 3 ​ C + 4 H → 3 Fe + CH 4 ​ ), trapping high-pressure methane at grain boundaries and causing catastrophic fissuring; safe operating boundaries for carbon and low-alloy steels are strictly governed by API RP 941 Nelson Curves.

Last updated: September 2026

16.2 Corrosion Mechanisms, Materials Degradation, and Prevention

Corrosion represents one of the largest single operational costs and safety risks in the chemical process industries (CPI), accounting for billions of dollars annually in premature equipment replacement, unscheduled outages, toxic releases, and fires. Chemical engineers must be able to diagnose corrosion failure modes, calculate metal loss rates, select appropriate alloys, and design cathodic or chemical mitigation systems. On the NCEES PE Chemical Exam , corrosion questions encompass electrochemical thermodynamics, rate kinetics, localized attack phenomena, environmental cracking, and standard industry guidelines (such as NACE/AMPP standards and API Recommended Practices).

  • 1. Electrochemical Foundations of Aqueous Corrosion
  • Anodic and Cathodic Half-Cell Reactions

Aqueous corrosion is an electrochemical process involving the transfer of electrons across a metal-solution interface. The process requires four components: an anode , a cathode , an electrolyte (ionic conductor), and a metallic path (electronic conductor). Removing any one of these four stops the corrosion process completely. Metallic Conductor (Electron Flow: e- --->)

  • ===============================================================
  • ANODE (-) CATHODE (+)
  • M -> M^(n+) + n e- 2 H+ + 2 e- -> H2 (Acid)
  • (Metal Dissolution Loss) O2 + 2 H2O + 4 e- -> 4 OH- (Base)
  • --------------------------------------------------------------
  • ELECTROLYTE (Ionic Solution)
  • Current Flow: Ions (M^(n+), OH-)

Anodic Reaction (Oxidation): Metal atoms lose electrons and dissolve into the electrolyte as cations: M ⟶ M n + + n e − ( Metal Loss / Dissolution ) M \longrightarrow M^{n+} + n e^-\qquad (\text{Metal Loss / Dissolution}) M ⟶ M n + + n e − ( Metal Loss / Dissolution )

  • Iron dissolution: Fe ⟶ Fe 2 + + 2 e − \text{Fe} \longrightarrow \text{Fe}^{2+} + 2e^- Fe ⟶ Fe 2 + + 2 e −
  • Aluminum dissolution: Al ⟶ Al 3 + + 3 e − \text{Al} \longrightarrow \text{Al}^{3+} + 3e^- Al ⟶ Al 3 + + 3 e −

Cathodic Reaction (Reduction): Electrons liberated at the anode travel through the metal to cathodic sites where they are consumed by reducible chemical species in solution. Common cathodic reactions in chemical plants include:

Hydrogen Evolution (Deaerated Acids, pH < 7 \text{pH} < 7 pH < 7 ): 2 H + + 2 e − ⟶ H 2 ↑ 2\text{H}^+ + 2e^- \longrightarrow \text{H}_2 \uparrow 2 H + + 2 e − ⟶ H 2 ​ ↑

Oxygen Reduction (Aerated Acidic Solutions): O 2 + 4 H + + 4 e − ⟶ 2 H 2 O \text{O}_2 + 4\text{H}^+ + 4e^- \longrightarrow 2\text{H}_2\text{O} O 2 ​ + 4 H + + 4 e − ⟶ 2 H 2 ​ O

Oxygen Reduction (Aerated Neutral or Alkaline Solutions, Cooling Water): O 2 + 2 H 2 O + 4 e − ⟶ 4 OH − \text{O}_2 + 2\text{H}_2\text{O} + 4e^- \longrightarrow 4\text{OH}^- O 2 ​ + 2 H 2 ​ O + 4 e − ⟶ 4 OH −

Water Reduction (Deaerated Neutral or Alkaline Solutions): 2 H 2 O + 2 e − ⟶ H 2 ↑ + 2 OH − 2\text{H}_2\text{O} + 2e^- \longrightarrow \text{H}_2 \uparrow + 2\text{OH}^- 2 H 2 ​ O + 2 e − ⟶ H 2 ​ ↑ + 2 OH −

The Nernst Equation & Thermodynamics

The reversible electrochemical potential (E) of a half-cell reaction at non-standard conditions is governed by the Nernst Equation : E = E ∘ − R T n F ln ⁡ Q = E ∘ − 2.3026 R T n F log ⁡ 10 Q E = E^\circ - \frac{R T}{n F} \ln Q = E^\circ - \frac{2.3026 R T}{n F} \log_{10} Q E = E ∘ − n F RT ​ ln Q = E ∘ − n F 2.3026 RT ​ lo g 10 ​ Q

At standard ambient conditions ( 25 ∘ C = 298.15 K 25^\circ\text{C} = 298.15\text{ K} 2 5 ∘ C = 298.15 K ): E = E ∘ − 0.05916 n log ⁡ 10 ( [ Red ] b [ Ox ] a ) E = E^\circ - \frac{0.05916}{n} \log_{10} \left( \frac{[\text{Red}]^b}{[\text{Ox}]^a} \right) E = E ∘ − n 0.05916 ​ lo g 10 ​ ( [ Ox ] a [ Red ] b ​ )

Where E ∘ E^\circ E ∘ is the standard reduction potential versus the Standard Hydrogen Electrode (SHE), (n) is the number of moles of electrons transferred, (F) is Faraday's constant ( 96 , 485 C/mol e − 96,485\text{ C/mol } e^- 96 , 485 C/mol e − ), and (Q) is the reaction quotient.

Pourbaix ( E -pH E\text{-pH} E -pH ) Diagrams

A Pourbaix diagram maps the thermodynamically stable phases of a metal-water system as a function of electrochemical potential ((E)) and solution pH \text{pH} pH : Potential E (V vs. SHE)

  • ^
  • +1.2 | (Oxygen Evolution Line b: O2 + 4H+ + 4e- = 2H2O)
  • | CORROSION PASSIVATION
  • | (Fe^3+) (Fe2O3 Passive Oxide Film)
  • 0.0 |------------------------------------------------------------
  • | (Fe^2+)
  • | CORROSION (Fe3O4 Magnetite Film)
  • 0.4 |------------------------+-----------------------------------
  • | (Hydrogen Line a: 2H+ + 2e- = H2)
  • 1.0 | IMMUNITY
  • | (Elemental Fe Stable, No Dissolution)
  • +------------------------+-----------------------------------> pH
  • 0 7 14

Immunity Zone: Potential is sufficiently negative that metal dissolution is thermodynamically impossible; the metal remains in its elemental state. This is the operating principle of Cathodic Protection .

Corrosion Zone: Soluble metal cations (e.g., Fe 2 + , Fe 3 + , Al 3 + \text{Fe}^{2+}, \text{Fe}^{3+}, \text{Al}^{3+} Fe 2 + , Fe 3 + , Al 3 + ) are thermodynamically stable, resulting in active metal dissolution and wall loss.

Passivation Zone: Insoluble, protective oxide or hydroxide films (e.g., Fe 2 O 3 , Cr 2 O 3 , TiO 2 , Al 2 O 3 \text{Fe}_2\text{O}_3, \text{Cr}_2\text{O}_3, \text{TiO}_2, \text{Al}_2\text{O}_3 Fe 2 ​ O 3 ​ , Cr 2 ​ O 3 ​ , TiO 2 ​ , Al 2 ​ O 3 ​ ) are thermodynamically stable. These films form a thin ( 1 − 5 nm 1 - 5\text{ nm} 1 − 5 nm ), non-porous barrier that stifles ionic diffusion, reducing corrosion current density by orders of magnitude.

  • 2. Uniform Corrosion & Corrosion Penetration Rate (CPR)
  • The CPR Equation

Uniform (general) corrosion is the even, distributed loss of metal across the entire exposed surface. The Corrosion Penetration Rate (CPR) represents the thickness of metal consumed per unit time, derived from mass-loss coupon testing: CPR = K Δ W ρ A t \text{CPR} = \frac{K \Delta W}{\rho A t} CPR = ρ A t K Δ W ​

Where:

Δ W \Delta W Δ W = mass loss of the test coupon during exposure time (t).

ρ \rho ρ = metal mass density ( g/cm 3 \text{g/cm}^3 g/cm 3 ; e.g., carbon steel ρ = 7.85 g/cm 3 \rho = 7.85\text{ g/cm}^3 ρ = 7.85 g/cm 3 , 316L SS ρ = 8.00 g/cm 3 \rho = 8.00\text{ g/cm}^3 ρ = 8.00 g/cm 3 , titanium ρ = 4.51 g/cm 3 \rho = 4.51\text{ g/cm}^3 ρ = 4.51 g/cm 3 ).

(A) = total exposed surface area.

(t) = exposure time in hours .

(K) = dimensional constant determined by target units: For CPR in m p y (mils per year, where 1 mil = 0.001 in ) : K = 534 ( Δ W in m g , ρ in g / c m 3 , A in i n 2 , t in h r ) For CPR in m m / y r (millimeters per year) : K = 87.6 ( Δ W in m g , ρ in g / c m 3 , A in c m 2 , t in h r ) \begin{aligned}

\text{For CPR in } \mathbf{mpy} \text{ (mils per year, where } 1\text{ mil} = 0.001\text{ in}): & \quad K = 534 \quad (\Delta W \text{ in } \mathbf{mg}, \rho \text{ in } \mathbf{g/cm}^3, A \text{ in } \mathbf{in}^2, t \text{ in } \mathbf{hr}) \\

\text{For CPR in } \mathbf{mm/yr} \text{ (millimeters per year)}: & \quad K = 87.6 \quad (\Delta W \text{ in } \mathbf{mg}, \rho \text{ in } \mathbf{g/cm}^3, A \text{ in } \mathbf{cm}^2, t \text{ in } \mathbf{hr})

\end{aligned} For CPR in mpy (mils per year, where 1 mil = 0.001 in ) : For CPR in mm/yr (millimeters per year) : ​ K = 534 ( Δ W in mg , ρ in g/cm 3 , A in in 2 , t in hr ) K = 87.6 ( Δ W in mg , ρ in g/cm 3 , A in cm 2 , t in hr ) ​

Unit Conversion: 1.0 mm/yr = 39.37 mpy ⟺ 1.0 mpy = 0.0254 mm/yr = 25.4 μ m/yr 1.0\text{ mm/yr} = 39.37\text{ mpy} \iff 1.0\text{ mpy} = 0.0254\text{ mm/yr} = 25.4\;\mu\text{m/yr} 1.0 mm/yr = 39.37 mpy ⟺ 1.0 mpy = 0.0254 mm/yr = 25.4 μ m/yr

Faraday's Law Link: Current Density to Corrosion Rate

By Faraday's Law , the mass loss rate is directly proportional to the corrosion current ( I corr I_{\text{corr}} I corr ​ ) or corrosion current density ( i corr = I corr / A i_{\text{corr}} = I_{\text{corr}} / A i corr ​ = I corr ​ / A ): CPR = C F ⋅ i corr ⋅ EW ρ \text{CPR} = \frac{C_F \cdot i_{\text{corr}} \cdot \text{EW}}{\rho} CPR = ρ C F ​ ⋅ i corr ​ ⋅ EW ​

Where i corr i_{\text{corr}} i corr ​ is in μ A/cm 2 \mu\text{A/cm}^2 μ A/cm 2 , ρ \rho ρ is in g/cm 3 \text{g/cm}^3 g/cm 3 , EW \text{EW} EW is the equivalent weight of the alloy ( EW = M / n \text{EW} = M/n EW = M / n , in g/equivalent \text{g/equivalent} g/equivalent ), and C F = 0.129 C_F = 0.129 C F ​ = 0.129 when CPR \text{CPR} CPR is in mpy (or C F = 0.00327 C_F = 0.00327 C F ​ = 0.00327 for mm/yr ).

Industrial Acceptability Guidelines

< 1.0 mpy ( < 0.025 mm/yr ) < 1.0\text{ mpy} \; (< 0.025\text{ mm/yr}) < 1.0 mpy ( < 0.025 mm/yr ) : Outstanding corrosion resistance. Essential for critical parts, valve trim, instrumentation, and thin heat exchanger tubes.

1.0 − 5.0 mpy ( 0.025 − 0.125 mm/yr ) 1.0 - 5.0\text{ mpy} \; (0.025 - 0.125\text{ mm/yr}) 1.0 − 5.0 mpy ( 0.025 − 0.125 mm/yr ) : Excellent resistance. Standard service for pressure vessels, tanks, and piping with standard corrosion allowances.

5.0 − 20.0 mpy ( 0.125 − 0.50 mm/yr ) 5.0 - 20.0\text{ mpy} \; (0.125 - 0.50\text{ mm/yr}) 5.0 − 20.0 mpy ( 0.125 − 0.50 mm/yr ) : Moderate resistance. Usable for short service lives or non-critical piping with heavy corrosion allowance.

> 20.0 mpy ( > 0.50 mm/yr ) > 20.0\text{ mpy} \; (> 0.50\text{ mm/yr}) > 20.0 mpy ( > 0.50 mm/yr ) : Unacceptable. Rapid failure, severe fouling, and product contamination.

  • 3. Galvanic Corrosion & The Area Ratio Effect
  • Mechanism & Galvanic Series

When two electrochemically dissimilar metals are in direct electrical contact within an electrolyte, the potential difference creates a galvanic couple:

The more active (less noble) metal becomes the anode and suffers accelerated galvanic corrosion.

The more noble (more positive) metal becomes the cathode and is galvanically protected from corrosion.

The driving force is established by the Galvanic Series in Seawater (more practical than the standard EMF series because it accounts for actual passivity): A c t i v e ( A n o d i c ) : Magnesium > Zinc > Aluminum 7075 > Carbon Steel > Cast Iron > Stainless Steel (Active) > Lead > Tin > Copper > Monel 400 N o b l e ( C a t h o d i c ) : > Stainless Steel (Passive) > Inconel 625 > Hastelloy C-276 > Titanium > Platinum > Graphite \begin{aligned}

\mathbf{Active \; (Anodic)}: & \quad \text{Magnesium} > \text{Zinc} > \text{Aluminum 7075} > \text{Carbon Steel} > \text{Cast Iron} \\

& \quad > \text{Stainless Steel (Active)} > \text{Lead} > \text{Tin} > \text{Copper} > \text{Monel 400} \\

\mathbf{Noble \; (Cathodic)}: & \quad > \text{Stainless Steel (Passive)} > \text{Inconel 625} > \text{Hastelloy C-276} > \text{Titanium} > \text{Platinum} > \text{Graphite}

\end{aligned} Active ( Anodic ) : Noble ( Cathodic ) : ​ Magnesium > Zinc > Aluminum 7075 > Carbon Steel > Cast Iron > Stainless Steel (Active) > Lead > Tin > Copper > Monel 400 > Stainless Steel (Passive) > Inconel 625 > Hastelloy C-276 > Titanium > Platinum > Graphite ​

The Critical Cathode-to-Anode Area Ratio

Conservation of electric charge dictates that the total anodic current must equal the total cathodic current: I A = I C I_A = I_C I A ​ = I C ​ . Expressed in current densities ((i = I/A)): ∋ A A A = i C A C ⟹ i A = i C ( A C A A ) \ni_A A_A = i_C A_C \implies i_A = i_C \left( \frac{A_C}{A_A} \right) ∋ A ​ A A ​ = i C ​ A C ​ ⟹ i A ​ = i C ​ ( A A ​ A C ​ ​ ) CASE 1: DISASTER (Large Cathode / Small Anode)

  • +--------------------------------------------------------------+
  • | LARGE CATHODE (Stainless Steel Plate, Area Ac = 100) |
  • +------------------------------+--+----------------------------+
  • |xx| <--- SMALL ANODE (Carbon Steel Rivet, Area Aa = 1)

Penetration Rate = i_c * (100 / 1) = 100x !

  • CASE 2: BENIGN (Small Cathode / Large Anode)
  • +--------------------------------------------------------------+
  • | LARGE ANODE (Carbon Steel Plate, Area Aa = 100) |
  • +------------------------------+--+----------------------------+
  • |oo| <--- SMALL CATHODE (Stainless Steel Fastener, Area Ac = 1)
  • Galvanic Acceleration = i_c * (1 / 100) = 0.01x (Negligible)

Caution

The Golden Rule of Galvanic Design:

NEVER couple a small anode to a large cathode! A carbon steel rivet or weld bead holding stainless steel plates in seawater will perforate in weeks (100× acceleration). Conversely, stainless steel fasteners holding large carbon steel plates produce negligible galvanic acceleration because the cathodic current is dispersed over a vast anodic area.

  • 4. Localized Corrosion: Pitting, Crevice, and PREN
  • Pitting Corrosion & Autocatalytic Acidification

Pitting is an extremely insidious form of localized attack where passive films locally break down in the presence of halides (especially chlorides, Cl − \text{Cl}^- Cl − ), forming deep, narrow holes while the surrounding surface remains completely unattacked.

Once a pit initiates, it grows by a self-sustaining autocatalytic mechanism : Bulk Solution (Aerated, Neutral pH ~ 7)

  • O2 + 2 H2O + 4 e- -> 4 OH- (Cathode)
  • ==================== ==================== (Passive Film)
  • Metal Surface \ / Metal Surface
  • \ +-------+ /
  • \ | Cl- | /
  • \ | Migr. | v /
  • \ +-------+ /
  • | |
  • | Anode: |
  • | M -> M+ + e-|
  • +-------------+

Inside Pit: Hydrolysis creates HCl !

M+ + Cl- + H2O -> MOH + H+ + Cl-

Local pH drops to 1 - 2 !

Inside the pit, metal rapidly oxidizes: Fe ⟶ Fe 2 + + 2 e − \text{Fe} \longrightarrow \text{Fe}^{2+} + 2e^- Fe ⟶ Fe 2 + + 2 e − .

Because the pit mouth is narrow, stagnant fluid prevents dissolved oxygen from replenishing inside the pit. Cathodic reduction of oxygen shifts to the exterior surface.

The concentrated build-up of positive Fe 2 + \text{Fe}^{2+} Fe 2 + ions attracts negative chloride ions ( Cl − \text{Cl}^- Cl − ) from the bulk solution to maintain electroneutrality.

Hydrolysis occurs inside the pit: Fe 2 + + 2 H 2 O + 2 Cl − ⟶ Fe ( OH ) 2 ↓ + 2 H + + 2 Cl − \text{Fe}^{2+} + 2\text{H}_2\text{O} + 2\text{Cl}^- \longrightarrow \text{Fe}(\text{OH})_2 \downarrow + 2\text{H}^+ + 2\text{Cl}^- Fe 2 + + 2 H 2 ​ O + 2 Cl − ⟶ Fe ( OH ) 2 ​ ↓ + 2 H + + 2 Cl −

Generation of free H + \text{H}^+ H + and Cl − \text{Cl}^- Cl − produces concentrated hydrochloric acid ( HCl \text{HCl} HCl ) , driving local pit pH \text{pH} pH down to (1.0 - 2.0) . The acidic chloride environment permanently destroys passivity, drilling rapidly through the vessel wall.

Pitting Resistance Equivalent Number (PREN)

Resistance to localized pitting and crevice attack in chloride environments is quantified by empirical alloy composition: PREN = % Cr + 3.3 ( % Mo ) + 16 ( % N ) \text{PREN} = \% \text{Cr} + 3.3 (\% \text{Mo}) + 16 (\% \text{N}) PREN = % Cr + 3.3 ( % Mo ) + 16 ( % N )

(In some duplex specifications, the nitrogen factor is 30: PREN 30 = % Cr + 3.3 % Mo + 30 % N \text{PREN}_{30} = \% \text{Cr} + 3.3\% \text{Mo} + 30\% \text{N} PREN 30 ​ = % Cr + 3.3% Mo + 30% N . The factor 16 is standard in NCEES specifications).

Type 304 SS (18Cr-8Ni-0Mo): PREN ≈ 18 − 20 \text{PREN} \approx 18 - 20 PREN ≈ 18 − 20 . Prone to pitting in tap water containing > 200 ppm > 200\text{ ppm} > 200 ppm chlorides.

Type 316L SS (17Cr-12Ni-2.5Mo): PREN ≈ 23 − 25 \text{PREN} \approx 23 - 25 PREN ≈ 23 − 25 . Resists chlorides up to 1 , 000 ppm 1,000\text{ ppm} 1 , 000 ppm at ambient temperature.

Duplex 2205 (22Cr-5Ni-3Mo-0.18N): PREN ≈ 35 \text{PREN} \approx 35 PREN ≈ 35 . Excellent resistance in brackish water.

Super Duplex 2507 & 6% Mo Super-Austenitics (AL-6XN, 254 SMO): PREN ≥ 40 − 45 \text{PREN} \ge 40 - 45 PREN ≥ 40 − 45 . Seawater service and warm chlorinated brine require PREN ≥ 40 \text{PREN} \ge 40 PREN ≥ 40 to prevent localized pitting.

Crevice Corrosion

Crevice corrosion occurs in narrow, stagnant geometries ( w < 100 μ m w < 100\;\mu\text{m} w < 100 μ m ) such as gasket flange faces, threaded connections, beneath tube-sheet roll expansions, or under sedimentary deposits. The mechanism mirrors pitting: oxygen within the micro-gap is quickly consumed, establishing a differential aeration cell. Chloride migration and subsequent hydrolysis create acidic HCl \text{HCl} HCl , causing aggressive localized metal dissolution. The Critical Crevice Temperature (CCT) is typically 20 − 30 ∘ C 20 - 30^\circ\text{C} 20 − 3 0 ∘ C lower than the Critical Pitting Temperature (CPT).

5. Environmental Cracking & Metallurgical Degradation +-------------------------------------------------------------------------+

  • | Environmental Cracking Mechanisms |
  • +-------------------------------------------------------------------------+
  • | Stress Corrosion Cracking (SCC) -- Tensile Stress + Specific Chemical |
  • | - Chloride SCC ---------------- Austenitic SS (304/316) > 60°C (140°F)|
  • | - Caustic Embrittlement ------- Carbon steel in hot NaOH (> 50-80°C) |
  • | - Amine SCC ------------------- Carbon steel in acid gas treaters |
  • | - Polythionic Acid SCC -------- Sensitized SS in refinery turnarounds |
  • | Intergranular Corrosion (IGC) --- Cr-carbide precipitation (425-850°C) |
  • | Hydrogen Damage: |
  • | - Hydrogen Embrittlement ------ High strength steels, loss of ductility|
  • | - Hydrogen Blistering --------- H2 gas traps at internal laminations |
  • | - HTHA (Nelson Curves) -------- Fe3C + 4H -> CH4 fissuring at > 200°C |
  • +-------------------------------------------------------------------------+
  • Stress Corrosion Cracking (SCC)

SCC requires the simultaneous presence of three interdependent factors: (1) tensile stress (residual welding stress or operating pressure), (2) a susceptible alloy metallurgy , and (3) a specific corrosive chemical environment .

Chloride Stress Corrosion Cracking (CSCC):

Occurs in standard austenitic stainless steels (304, 304L, 316, 316L) exposed to aqueous chlorides.

Critical Temperature Threshold: Rarely occurs below 60 ∘ C ( 140 ∘ F ) 60^\circ\text{C} \; (140^\circ\text{F}) 6 0 ∘ C ( 14 0 ∘ F ) ; risk accelerates exponentially with higher temperature.

Morphology: Highly branched, transgranular cleavage cracks ("lightning bolt" pattern).

Mitigation: Upgrade to Duplex 2205, Super Duplex, or Nickel Alloy 625/825; or eliminate chlorides/reduce temperature.

Caustic Embrittlement (Caustic SCC):

Occurs in carbon steels exposed to concentrated sodium hydroxide ( NaOH \text{NaOH} NaOH ) at elevated temperatures ( > 50 − 80 ∘ C > 50 - 80^\circ\text{C} > 50 − 8 0 ∘ C ).

Morphology: Intergranular cracking along ferrite grain boundaries.

Mitigation: Perform mandatory Post-Weld Heat Treatment (PWHT) (stress-relieving at 600 − 650 ∘ C 600 - 650^\circ\text{C} 600 − 65 0 ∘ C per NACE SP0472), or upgrade to Nickel 200/201.

Amine Stress Corrosion Cracking:

Occurs in carbon steel alkanolamine gas treating units (MEA, DEA, MDEA) used to remove CO 2 \text{CO}_2 CO 2 ​ and H 2 S \text{H}_2\text{S} H 2 ​ S .

Mitigation: Strict adherence to API RP 945 , mandating full PWHT of all welded piping and vessels regardless of wall thickness.

Polythionic Acid SCC (PASCC):

Occurs during refinery turnarounds in hydroprocessing reactors fabricated from sensitized austenitic stainless steels. When sulfide scale ( FeS \text{FeS} FeS ) contacts oxygen and liquid water during shutdown, it oxidizes to polythionic acids ( H 2 S x O 6 \text{H}_2\text{S}_x\text{O}_6 H 2 ​ S x ​ O 6 ​ ), causing rapid intergranular cracking.

Mitigation: Follow NACE SP0170 (purge equipment with dry nitrogen or circulate a 1–2% soda ash [ Na 2 CO 3 \text{Na}_2\text{CO}_3 Na 2 ​ CO 3 ​ ] neutralization wash before admitting air).

Intergranular Corrosion (IGC) & Sensitization

As introduced in Section 16.1, heating standard austenitic stainless steels (e.g., 304, 316) between 425 ∘ C 425^\circ\text{C} 42 5 ∘ C and 850 ∘ C 850^\circ\text{C} 85 0 ∘ C ( 800 ∘ F − 1500 ∘ F 800^\circ\text{F} - 1500^\circ\text{F} 80 0 ∘ F − 150 0 ∘ F ) causes carbon to rapidly diffuse to grain boundaries, where it reacts with chromium to precipitate chromium carbide ( Cr 23 C 6 \text{Cr}_{23}\text{C}_6 Cr 23 ​ C 6 ​ ) . Because chromium diffuses vastly slower than carbon, chromium in the grain matrix adjacent to the boundary is depleted below 12 % 12\% 12% . In an acid electrolyte, this chromium-depleted boundary forms a microscopic active anode coupled to the massive cathodic grain interior, resulting in deep, rapid grain dislodgement ("sugaring" or "knife-line attack").

Hydrogen Damage Mechanisms

Hydrogen Embrittlement (HE): Atomic hydrogen ( H 0 \text{H}^0 H 0 ) generated during acid pickling, electroplating, or sour service ( H 2 S \text{H}_2\text{S} H 2 ​ S ) diffuses into high-strength steel lattices, pinning dislocations and causing brittle fracture under tensile stress.

Hydrogen Blistering: Atomic hydrogen diffuses through steel and encounters microscopic internal voids or manganese sulfide ( MnS \text{MnS} MnS ) inclusions. There, two hydrogen atoms recombine into molecular hydrogen gas ( 2 H ⟶ H 2 ↑ 2\text{H} \longrightarrow \text{H}_2 \uparrow 2 H ⟶ H 2 ​ ↑ ). Because molecular H 2 \text{H}_2 H 2 ​ is too large to diffuse out, internal gas pressure builds to thousands of atmospheres, plastically deforming the steel into surface blisters.

High-Temperature Hydrogen Attack (HTHA):

Occurs in carbon and low-alloy steels exposed to high hydrogen partial pressure ( P H 2 > 100 psia P_{\text{H}_2} > 100\text{ psia} P H 2 ​ ​ > 100 psia ) at elevated temperatures ( T > 200 ∘ C [ 400 ∘ F ] T > 200^\circ\text{C} \; [400^\circ\text{F}] T > 20 0 ∘ C [ 40 0 ∘ F ] ) in hydrocrackers, hydrotreaters, and ammonia converters.

Mechanism: Atomic hydrogen diffuses into steel and reacts with cementite (iron carbide): Fe 3 C + 4 H ⟶ 3 Fe + CH 4 ↑ \text{Fe}_3\text{C} + 4\text{H} \longrightarrow 3\text{Fe} + \text{CH}_4 \uparrow Fe 3 ​ C + 4 H ⟶ 3 Fe + CH 4 ​ ↑

Methane gas ( CH 4 \text{CH}_4 CH 4 ​ ) cannot diffuse out through the crystal lattice. Extreme methane pressure nucleates micro-fissures along grain boundaries, causing decarburization, loss of tensile strength, and catastrophic rupture.

API RP 941 Nelson Curves: Safe operating limits for process equipment are defined by empirical Nelson Curves , which establish maximum safe temperature and H 2 \text{H}_2 H 2 ​ partial pressure limits for carbon steel, 0.5 Mo 0.5\text{Mo} 0.5 Mo , 1.25 Cr − 0.5 Mo 1.25\text{Cr}-0.5\text{Mo} 1.25 Cr − 0.5 Mo , 2.25 Cr − 1 Mo 2.25\text{Cr}-1\text{Mo} 2.25 Cr − 1 Mo , and 3 Cr − 1 Mo 3\text{Cr}-1\text{Mo} 3 Cr − 1 Mo . Adding carbide-stabilizing elements (Cr, Mo, V) binds carbon into stable carbides (e.g., Cr 7 C 3 , Mo 2 C \text{Cr}_7\text{C}_3, \text{Mo}_2\text{C} Cr 7 ​ C 3 ​ , Mo 2 ​ C ) that resist methane formation.

6. Flow-Induced and Biological Degradation

Erosion-Corrosion: Acceleration in metal dissolution caused by high fluid velocity, turbulence, or impingement mechanically stripping the protective passive film. Most severe at pipe elbows, tees, orifices, and downstream of control valves. Characterized by directional grooves, waves, or "horseshoe" shaped depressions.

Cavitation: Occurs in high-speed centrifugal pumps and control valves where local pressure drops below vapor pressure, generating vapor bubbles. When these bubbles enter higher-pressure regions, they violently implode, generating localized micro-jets with shock pressures exceeding 1 , 000 MPa 1,000\text{ MPa} 1 , 000 MPa . This micro-hammering destroys passive films and mechanically fatigues metal.

Microbiologically Influenced Corrosion (MIC): Microorganisms establish metabolic colonies (biofilms) on metal surfaces, creating localized anaerobic micro-environments:

Sulfate-Reducing Bacteria (SRB, e.g., Desulfovibrio ): Under anaerobic conditions (water tanks, stagnant pipelines), SRBs consume cathodic hydrogen and reduce sulfate ions ( SO 4 2 − \text{SO}_4^{2-} SO 4 2 − ​ ) to sulfide ( S 2 − \text{S}^{2-} S 2 − ), producing highly corrosive hydrogen sulfide ( H 2 S \text{H}_2\text{S} H 2 ​ S ) and precipitating black iron sulfide ( FeS \text{FeS} FeS ) scale.

Acid-Producing Bacteria (APB): Secrete organic acids (acetic, butyric) that drive local pH \text{pH} pH under the biofilm down to (2 - 3).

7. Corrosion Prevention & Mitigation Engineering +-------------------------------------------------------------------------+

  • | Corrosion Prevention Strategies |
  • +-------------------------------------------------------------------------+
  • | Cathodic Protection: |
  • | - Sacrificial Anodes (SACP) --- Zn, Al, Mg (passive, no power) |
  • | - Impressed Current (ICCP) ---- DC rectifier, MMO/Pt anodes, large A |
  • | Chemical Inhibitors: |
  • | - Anodic (Passivating) -------- DANGEROUS if underdosed (Pitting!) |
  • | - Cathodic -------------------- Safe (suppresses reduction rate) |
  • | - Mixed / Film-Forming -------- Organic amines, hydrophobic film |
  • | Protective Coatings & Linings --- Epoxies, PTFE, rubber, glass |
  • +-------------------------------------------------------------------------+
  • Cathodic Protection (CP)

Cathodic protection polarizes the metal structure into the thermodynamic Immunity Zone of the Pourbaix diagram (potential E < − 0.850 V E < -0.850\text{ V} E < − 0.850 V versus a Copper/Copper Sulfate Electrode [CSE] for carbon steel in soil/water).

  • Feature Sacrificial Anode Cathodic Protection (SACP) Impressed Current Cathodic Protection (ICCP)
  • Power Source None (natural electrochemical galvanic cell) External AC-to-DC transformer-rectifier

Anode Materials Zinc (seawater), Aluminum alloys (marine), Magnesium (high-resistivity soils) Mixed Metal Oxide (MMO) coated titanium, Platinized titanium, High-Silicon Cast Iron

Driving Voltage Limited ( Δ E ≈ 0.2 − 0.7 V \Delta E \approx 0.2 - 0.7\text{ V} Δ E ≈ 0.2 − 0.7 V ) High and adjustable ( 10 − 50 V 10 - 50\text{ V} 10 − 50 V )

Current Output Low (typically < 1 − 5 A < 1 - 5\text{ A} < 1 − 5 A ) High ( 10 − 200 + A 10 - 200+\text{ A} 10 − 200 + A )

Application Scope Small structures, offshore jackets, buried storage tanks, heat exchanger water boxes Cross-country pipelines, large storage tank bottoms, marine docks

  • Maintenance Minimal; inspect anode consumption Continuous monitoring; potential stray current interference
  • Chemical Corrosion Inhibitors

Chemical inhibitors are substances added in small concentrations ( 10 − 500 ppm 10 - 500\text{ ppm} 10 − 500 ppm ) to process streams to suppress corrosion rates:

Anodic Inhibitors (Passivators): Oxidizing anions (nitrites [ NO 2 − ] [\text{NO}_2^-] [ NO 2 − ​ ] , chromates [ CrO 4 2 − ] [\text{CrO}_4^{2-}] [ CrO 4 2 − ​ ] , orthophosphates) that shift the corrosion potential positive into the passive region, strengthening the oxide barrier.

Warning

High-Risk PE Exam Trap: Anodic inhibitors are dangerous inhibitors ! If an anodic inhibitor is underdosed, passivity is established over most of the surface but fails at small bare spots, creating a small active anode coupled to a massive passivated cathode . This causes severe, accelerated localized pitting that perforates equipment faster than if no inhibitor were added at all!

Cathodic Inhibitors: Substances that precipitate insoluble protective films at cathodic sites where alkaline OH − \text{OH}^- OH − ions are generated (e.g., zinc salts [ Zn 2 + ] [\text{Zn}^{2+}] [ Zn 2 + ] , calcium bicarbonate, polyphosphates). They are safe inhibitors because underdosing never accelerates localized attack; it simply provides partial uniform protection.

Mixed / Organic Film-Forming Inhibitors: Long-chain aliphatic amines or imidazolines containing polar nitrogen groups that adsorb onto metal surfaces, with long hydrophobic hydrocarbon tails projecting outward into the fluid to repel water, acids, and ions.

  • 8. Summary Comparison Tables
  • Table 1: Major Degradation Mechanisms, Susceptible Alloys, and Solutions

Degradation Mechanism Characteristic Environment Highly Susceptible Alloys Primary Mitigation Method

Uniform Corrosion Acidic or aerated process streams Carbon Steel, Cast Iron Apply corrosion allowance ( CA \text{CA} CA ), chemical inhibitors, protective coatings

Galvanic Corrosion Electrolyte coupling dissimilar metals Active metal in couple (e.g., Carbon steel riveted to Stainless) Electrical isolation gaskets/sleeves; avoid small anode/large cathode ratio

Pitting & Crevice Aqueous chlorides, stagnant deadlegs Austenitic 304/316 SS Select high-PREN alloys ( PREN ≥ 40 \text{PREN} \ge 40 PREN ≥ 40 ), eliminate crevice geometries

Chloride SCC Chlorides at T > 60 ∘ C ( 140 ∘ F ) T > 60^\circ\text{C} \; (140^\circ\text{F}) T > 6 0 ∘ C ( 14 0 ∘ F ) Austenitic 304, 304L, 316, 316L Upgrade to Duplex 2205, Super Duplex, or Nickel Alloy 625

Caustic Embrittlement NaOH > 50 − 80 ∘ C \text{NaOH} > 50 - 80^\circ\text{C} NaOH > 50 − 8 0 ∘ C Carbon Steel Post-Weld Heat Treatment (PWHT); upgrade to Nickel 200/201

Amine SCC Alkanolamine gas sweetening As-welded Carbon Steel Full PWHT per API RP 945

Sensitization / IGC Welded heat-affected zones High-carbon austenitic SS (304, 316) Low-carbon L-grades (304L, 316L), stabilized grades (321, 347), solution anneal

HTHA H 2 H_2 H 2 ​ partial pressure > 100 psi > 100\text{ psi} > 100 psi , T > 200 ∘ C T > 200^\circ\text{C} T > 20 0 ∘ C Carbon Steel, C-0.5Mo Select Cr-Mo steels per API RP 941 Nelson Curves

Erosion-Corrosion High velocity slurries, pipe bends Soft alloys (Copper, Carbon Steel) Increase pipe diameter, use hardened alloys (Stellite), sweep elbows

MIC Stagnant cooling water, wet soils Carbon Steel, 304 SS Biocide shock treatment (bleach, glutaraldehyde), eliminate deadlegs, pigging

  • 9. Comprehensive Worked Numerical Example
  • Problem Statement

A refinery sour water stripper overhead condenser experiences accelerated degradation. Solve the following three engineering evaluations:

Corrosion Penetration Rate & Pipeline Remaining Life: An ASTM A106 Grade B carbon steel corrosion coupon ( ρ = 7.85 g/cm 3 \rho = 7.85\text{ g/cm}^3 ρ = 7.85 g/cm 3 ) is installed in the overhead vapor line. The coupon has outer dimensions of 2.00 in × 1.00 in × 0.125 in 2.00\text{ in} \times 1.00\text{ in} \times 0.125\text{ in} 2.00 in × 1.00 in × 0.125 in with a central mounting hole of diameter d = 0.250 in d = 0.250\text{ in} d = 0.250 in . After 2 , 160 hours 2,160\text{ hours} 2 , 160 hours ( 90.0 days 90.0\text{ days} 90.0 days ) of steady service, the coupon is removed, cleaned of scale, and reweighed. The initial weight was W 1 = 31.850 g W_1 = 31.850\text{ g} W 1 ​ = 31.850 g and the final cleaned weight is W 2 = 29.425 g W_2 = 29.425\text{ g} W 2 ​ = 29.425 g . Determine the total exposed surface area (A) in in 2 \text{in}^2 in 2 , the mass loss Δ W \Delta W Δ W in mg \text{mg} mg , the Corrosion Penetration Rate ( CPR \text{CPR} CPR ) in mils per year ( mpy \text{mpy} mpy ), and CPR \text{CPR} CPR in mm/yr \text{mm/yr} mm/yr . If the overhead carbon steel transfer line has a current ultrasonic measured wall thickness of 0.310 in 0.310\text{ in} 0.310 in and an ASME BPVC minimum allowable retirement thickness of t min = 0.200 in t_{\text{min}} = 0.200\text{ in} t min ​ = 0.200 in , calculate the remaining operational lifetime of the line in years assuming this corrosion rate continues.

Galvanic Area Ratio Acceleration: The condenser features titanium tubes ( A C = 20.0 ft 2 A_C = 20.0\text{ ft}^2 A C ​ = 20.0 ft 2 ) rolled into a carbon steel channel shell. A small carbon steel weld fillet ( A A = 0.50 ft 2 A_A = 0.50\text{ ft}^2 A A ​ = 0.50 ft 2 , ρ = 7.85 g/cm 3 \rho = 7.85\text{ g/cm}^3 ρ = 7.85 g/cm 3 , EW = 27.92 g/equivalent \text{EW} = 27.92\text{ g/equivalent} EW = 27.92 g/equivalent ) is exposed to aerated cooling water. The cathodic oxygen reduction current density on the titanium surface is i C = 15.0 μ A/cm 2 i_C = 15.0\;\mu\text{A/cm}^2 i C ​ = 15.0 μ A/cm 2 . Assuming the couple is under complete cathodic control, calculate the accelerated anodic current density i A i_A i A ​ on the carbon steel weld in μ A/cm 2 \mu\text{A/cm}^2 μ A/cm 2 , and the resulting galvanic penetration rate in mpy \text{mpy} mpy and mm/yr \text{mm/yr} mm/yr .

PREN Evaluation for Cooling Water Alloy Selection: Brackish estuarine cooling water containing 15 , 000 ppm 15,000\text{ ppm} 15 , 000 ppm chlorides at 38 ∘ C 38^\circ\text{C} 3 8 ∘ C is used. Compute the PREN for Type 316L SS (17.0% Cr, 2.1% Mo, 0.04% N), Duplex 2205 (22.0% Cr, 3.1% Mo, 0.18% N), and Super Duplex 2507 (25.0% Cr, 4.0% Mo, 0.28% N). Determine which alloy satisfies the marine threshold of PREN ≥ 40 \text{PREN} \ge 40 PREN ≥ 40 .

Step 1: Corrosion Coupon CPR & Remaining Life

First calculate the exposed surface area (A) of the rectangular coupon with mounting hole:

Two main rectangular faces: 2 × ( 2.00 × 1.00 ) = 4.000 in 2 2 \times (2.00 \times 1.00) = 4.000\text{ in}^2 2 × ( 2.00 × 1.00 ) = 4.000 in 2 .

Two long edge faces: 2 × ( 2.00 × 0.125 ) = 0.500 in 2 2 \times (2.00 \times 0.125) = 0.500\text{ in}^2 2 × ( 2.00 × 0.125 ) = 0.500 in 2 .

Two short edge faces: 2 × ( 1.00 × 0.125 ) = 0.250 in 2 2 \times (1.00 \times 0.125) = 0.250\text{ in}^2 2 × ( 1.00 × 0.125 ) = 0.250 in 2 .

Mounting hole correction: Area subtracted from two faces = − 2 × ( π 4 d 2 ) = − 2 × ( π 4 ( 0.250 ) 2 ) = − 0.09817 in 2 \text{Area subtracted from two faces} = -2 \times \left( \frac{\pi}{4} d^2 \right) = -2 \times \left( \frac{\pi}{4} (0.250)^2 \right) = -0.09817\text{ in}^2 Area subtracted from two faces = − 2 × ( 4 π ​ d 2 ) = − 2 × ( 4 π ​ ( 0.250 ) 2 ) = − 0.09817 in 2 Cylindrical inside hole area added = + π d t h = π ( 0.250 ) ( 0.125 ) = + 0.09817 in 2 \text{Cylindrical inside hole area added} = +\pi d t_h = \pi (0.250) (0.125) = +0.09817\text{ in}^2 Cylindrical inside hole area added = + π d t h ​ = π ( 0.250 ) ( 0.125 ) = + 0.09817 in 2 (Notice: The hole face area subtracted exactly equals the cylindrical bore area added!)

Total exposed surface area: A = 4.000 + 0.500 + 0.250 = 4.750 in 2 A = 4.000 + 0.500 + 0.250 = \mathbf{4.750\text{ in}^2} A = 4.000 + 0.500 + 0.250 = 4.750 in 2

Compute mass loss: Δ W = W 1 − W 2 = 31.850 g − 29.425 g = 2.425 g = 2 , 425.0 mg \Delta W = W_1 - W_2 = 31.850\text{ g} - 29.425\text{ g} = 2.425\text{ g} = \mathbf{2,425.0\text{ mg}} Δ W = W 1 ​ − W 2 ​ = 31.850 g − 29.425 g = 2.425 g = 2 , 425.0 mg

Compute Corrosion Penetration Rate in mpy \text{mpy} mpy using (K = 534): CPR = K Δ W ρ A t = 534 × 2425.0 mg ( 7.85 g/cm 3 ) × ( 4.750 in 2 ) × ( 2160 hr ) \text{CPR} = \frac{K \Delta W}{\rho A t} = \frac{534 \times 2425.0\text{ mg}}{(7.85\text{ g/cm}^3) \times (4.750\text{ in}^2) \times (2160\text{ hr})} CPR = ρ A t K Δ W ​ = ( 7.85 g/cm 3 ) × ( 4.750 in 2 ) × ( 2160 hr ) 534 × 2425.0 mg ​ Numerator = 534 × 2425.0 = 1 , 294 , 950 \text{Numerator} = 534 \times 2425.0 = 1,294,950 Numerator = 534 × 2425.0 = 1 , 294 , 950 Denominator = 7.85 × 4.750 × 2160 = 80 , 541 \text{Denominator} = 7.85 \times 4.750 \times 2160 = 80,541 Denominator = 7.85 × 4.750 × 2160 = 80 , 541 CPR = 1 , 294 , 950 80 , 541 = 16.078 mpy ≈ 16.1 mpy \text{CPR} = \frac{1,294,950}{80,541} = \mathbf{16.078\text{ mpy}} \approx 16.1\text{ mpy} CPR = 80 , 541 1 , 294 , 950 ​ = 16.078 mpy ≈ 16.1 mpy

Convert to mm/yr \text{mm/yr} mm/yr : CPR = 16.078 mpy × 0.0254 mm/(mpy) = 0.4084 mm/yr \text{CPR} = 16.078\text{ mpy} \times 0.0254\text{ mm/(mpy)} = \mathbf{0.4084\text{ mm/yr}} CPR = 16.078 mpy × 0.0254 mm/(mpy) = 0.4084 mm/yr

Compute remaining allowable metal loss before reaching retirement thickness: Δ t allowable = t actual − t min = 0.310 in − 0.200 in = 0.110 in = 110.0 mils \Delta t_{\text{allowable}} = t_{\text{actual}} - t_{\text{min}} = 0.310\text{ in} - 0.200\text{ in} = 0.110\text{ in} = 110.0\text{ mils} Δ t allowable ​ = t actual ​ − t min ​ = 0.310 in − 0.200 in = 0.110 in = 110.0 mils

Calculate remaining service life: Remaining Life = Δ t allowable CPR = 110.0 mils 16.078 mpy = 6.84 years \text{Remaining Life} = \frac{\Delta t_{\text{allowable}}}{\text{CPR}} = \frac{110.0\text{ mils}}{16.078\text{ mpy}} = \mathbf{6.84\text{ years}} Remaining Life = CPR Δ t allowable ​ ​ = 16.078 mpy 110.0 mils ​ = 6.84 years

Step 2: Galvanic Acceleration on Carbon Steel Weld

Compute the cathode-to-anode area ratio: A C A A = 20.0 ft 2 0.50 ft 2 = 40.0 \frac{A_C}{A_A} = \frac{20.0\text{ ft}^2}{0.50\text{ ft}^2} = 40.0 A A ​ A C ​ ​ = 0.50 ft 2 20.0 ft 2 ​ = 40.0

Calculate accelerated anodic current density on the carbon steel weld: ∋ A = i C × ( A C A A ) = 15.0 μ A/cm 2 × 40.0 = 600.0 μ A/cm 2 \ni_A = i_C \times \left( \frac{A_C}{A_A} \right) = 15.0\;\mu\text{A/cm}^2 \times 40.0 = \mathbf{600.0\;\mu\text{A/cm}^2} ∋ A ​ = i C ​ × ( A A ​ A C ​ ​ ) = 15.0 μ A/cm 2 × 40.0 = 600.0 μ A/cm 2

Compute accelerated penetration rate via Faraday's equation: CPR A = 0.129 × i A × EW ρ = 0.129 × 600.0 × 27.92 7.85 \text{CPR}_A = \frac{0.129 \times i_A \times \text{EW}}{\rho} = \frac{0.129 \times 600.0 \times 27.92}{7.85} CPR A ​ = ρ 0.129 × i A ​ × EW ​ = 7.85 0.129 × 600.0 × 27.92 ​ Numerator = 0.129 × 600.0 × 27.92 = 2 , 161.01 \text{Numerator} = 0.129 \times 600.0 \times 27.92 = 2,161.01 Numerator = 0.129 × 600.0 × 27.92 = 2 , 161.01 CPR A = 2 , 161.01 7.85 = 275.3 mpy \text{CPR}_A = \frac{2,161.01}{7.85} = \mathbf{275.3\text{ mpy}} CPR A ​ = 7.85 2 , 161.01 ​ = 275.3 mpy CPR A in mm/yr = 275.3 × 0.0254 = 6.99 mm/yr \text{CPR}_A\text{ in mm/yr} = 275.3 \times 0.0254 = \mathbf{6.99\text{ mm/yr}} CPR A ​ in mm/yr = 275.3 × 0.0254 = 6.99 mm/yr

(Critical finding: The galvanic couple accelerates the corrosion rate from a tolerable 6.9 mpy 6.9\text{ mpy} 6.9 mpy baseline to a catastrophic 275.3 mpy 275.3\text{ mpy} 275.3 mpy , which would perforate a 0.375 in 0.375\text{ in} 0.375 in shell in under 1.4 years 1.4\text{ years} 1.4 years ).

Step 3: PREN Evaluation for Warm Estuarine Brine

Calculate PREN using PREN = % Cr + 3.3 ( % Mo ) + 16 ( % N ) \text{PREN} = \% \text{Cr} + 3.3(\% \text{Mo}) + 16(\% \text{N}) PREN = % Cr + 3.3 ( % Mo ) + 16 ( % N ) :

Type 316L SS: PREN = 17.0 + 3.3 ( 2.1 ) + 16 ( 0.04 ) = 17.0 + 6.93 + 0.64 = 24.57 \text{PREN} = 17.0 + 3.3(2.1) + 16(0.04) = 17.0 + 6.93 + 0.64 = \mathbf{24.57} PREN = 17.0 + 3.3 ( 2.1 ) + 16 ( 0.04 ) = 17.0 + 6.93 + 0.64 = 24.57

Duplex 2205: PREN = 22.0 + 3.3 ( 3.1 ) + 16 ( 0.18 ) = 22.0 + 10.23 + 2.88 = 35.11 \text{PREN} = 22.0 + 3.3(3.1) + 16(0.18) = 22.0 + 10.23 + 2.88 = \mathbf{35.11} PREN = 22.0 + 3.3 ( 3.1 ) + 16 ( 0.18 ) = 22.0 + 10.23 + 2.88 = 35.11

Super Duplex 2507: PREN = 25.0 + 3.3 ( 4.0 ) + 16 ( 0.28 ) = 25.0 + 13.20 + 4.48 = 42.68 \text{PREN} = 25.0 + 3.3(4.0) + 16(0.28) = 25.0 + 13.20 + 4.48 = \mathbf{42.68} PREN = 25.0 + 3.3 ( 4.0 ) + 16 ( 0.28 ) = 25.0 + 13.20 + 4.48 = 42.68

Conclusion: Only Super Duplex 2507 ( PREN = 42.68 ≥ 40 \text{PREN} = 42.68 \ge 40 PREN = 42.68 ≥ 40 ) satisfies the threshold required to eliminate pitting and crevice attack in chlorinated 15 , 000 ppm 15,000\text{ ppm} 15 , 000 ppm brackish water at 38 ∘ C 38^\circ\text{C} 3 8 ∘ C .

10. Critical PE Exam Traps & Pitfalls

  • Warning
  • Trap 1: Underdosing Anodic (Passivating) Inhibitors

The most heavily tested safety paradox on the PE exam is that underdosing an anodic corrosion inhibitor (such as sodium nitrite or chromate) is vastly more dangerous than adding nothing at all. An insufficient dose leaves microscopic unpassivated spots that act as tiny anodes coupled to a massive passivated cathode, accelerating localized pit penetration by orders of magnitude.

  • Warning
  • Trap 2: Area Ratio Inversion in Galvanic Calculations

When computing galvanic corrosion acceleration, candidates often invert the area ratio: i A = i C ( A C / A A ) i_A = i_C (A_C / A_A) i A ​ = i C ​ ( A C ​ / A A ​ ) , NOT i C ( A A / A C ) i_C (A_A / A_C) i C ​ ( A A ​ / A C ​ ) . Large cathode area over small anode area drives the multiplier up; small cathode over large anode reduces the galvanic effect.

  • Warning
  • Trap 3: CPR Units and Constants (534 vs. 87.6)

The dimensional constant (K = 534) applies only when CPR \text{CPR} CPR is in mpy , mass loss is in mg , and area is in in 2 \text{in}^2 in 2 . If using metric units (area in cm 2 \text{cm}^2 cm 2 and CPR \text{CPR} CPR in mm/yr ), you must use (K = 87.6) (for mass in mg \text{mg} mg ) or K = 3.45 × 10 6 K = 3.45 \times 10^6 K = 3.45 × 1 0 6 (for mass in g \text{g} g ). Mixing English area ( in 2 \text{in}^2 in 2 ) with (K = 87.6) is a common calculation trap.

  • Warning
  • Trap 4: Chloride SCC Temperature Cutoff in Austenitic Stainless Steels

Candidates frequently specify expensive titanium or nickel alloys for cold chloride brine streams where standard 304 or 316 would perform adequately. Remember that chloride SCC in 300-series stainless steels occurs almost exclusively at temperatures above 60 ∘ C ( 140 ∘ F ) 60^\circ\text{C} \; (140^\circ\text{F}) 6 0 ∘ C ( 14 0 ∘ F ) . Below 60 ∘ C 60^\circ\text{C} 6 0 ∘ C , 316L resists chloride SCC, provided pitting thresholds are respected.