Study guide

6.1 High-Cycle Fatigue, S-N Curves & Marin Modifying Factors

PE Mechanical: Machine Design and Materials Exam

Track your progress as you read

Finished sections get a check mark.

1 Chapter 1: Basic Engineering Practice: Drawings, Economics & Design Methodology

1.1 Engineering Terms, Symbols, Drawing Interpretation & Conventions 1.2 Project Management & Engineering Economics 1.3 Design Methodology, Risk Assessment & Safety

2 Chapter 2: Physical & Mechanical Properties of Engineering Materials

2.1 Stress-Strain Relationships & Fundamental Mechanical Properties 2.2 Physical Properties, Temperature Effects, Hardness, Impact Toughness & Creep

3 Chapter 3: Mechanics of Materials: Fundamental Loadings & Deflections

3.1 Axial Loading, Normal Stress & Statically Indeterminate Members 3.2 Direct Shear, Bearing & Transverse Shear in Beams 3.3 Torsion of Shafts, Power Transmission & Thin-Walled Tubes 3.4 Beam Bending Stresses & Deflection Analysis

4 Chapter 4: Mechanics of Materials: Stability, Multiaxial Stress & Thermal Effects

4.1 Column Buckling & Elastic/Inelastic Instability 4.2 Combined Loading, Principal Stresses & Mohr's Circle 4.3 Thermal Stresses & Interference Stresses

5 Chapter 5: Failure Theories: Static Yielding & Fracture Mechanics

5.1 Static Failure Theories for Ductile Materials: von Mises & Tresca 5.2 Static Failure Theories for Brittle Materials & Fracture Mechanics

6 Chapter 6: Fatigue Analysis & Dynamic Failure

6.1 High-Cycle Fatigue, S-N Curves & Marin Modifying Factors 6.2 Fluctuating Stresses, Failure Criteria & Cumulative Damage

7 Chapter 7: Mechanical Attachments: Fasteners & Bolted Joints

7.1 Threaded Fasteners, Proof Strength & Preload Mechanics 7.2 Bolted Joint Stiffness, External Loading & Separation 7.3 Non-Threaded Fasteners: Keys, Pins, Clevises, Retaining Rings, Rivets, Lugs & Anchors

8 Chapter 8: Mechanical Attachments: Permanent Joints & Bonding

8.1 Welded Joints & Weld Group Stress Analysis 8.2 Brazing, Soldering & Structural Adhesive Bonding

9 Chapter 9: Power Transmission: Shafts & Gearing

9.1 Transmission Shaft Design, Critical Speeds & Deflection 9.2 Spur Gears: Geometry, Kinematics & AGMA Stress Equations 9.3 Helical, Bevel & Worm Gearing

10 Chapter 10: Power Transmission: Bearings, Flexible Drives, Friction Devices & Prime Movers

10.1 Rolling-Element Bearings & L10 Life Calculations 10.2 Hydrodynamic Journal Bearings & Lubrication Regimes 10.3 Belts, Roller Chains & Flexible Drives 10.4 Clutches, Brakes & Power Screws 10.5 Electric Motors, Engines & Flywheels

11 Chapter 11: Mechanical Components: Pressure Vessels & Structural Systems

11.1 Pressure Vessels & Piping: Thin and Thick Walls, ASME VIII and B31 11.2 Mechanical Springs: Helical, Belleville & Leaf Springs 11.3 Structural Trusses, Rigid Frames & Energy Methods

12 Chapter 12: Mechanical Dynamics, Vibrations & Fluid Power

12.1 Single-Degree-of-Freedom Vibrations & Resonance 12.2 Vibration Isolation, Multi-DOF Systems & Transmissibility 12.3 Fluid Power Systems: Hydraulics & Pneumatics

13 Chapter 13: Kinematics, Mechatronics & Control Systems

13.1 Mechanism Kinematics, Linkages, Cams & Simple Machines 13.2 Basic Mechatronics, Sensors & Closed-Loop Controls

14 Chapter 14: Supportive Knowledge: Fits, Tolerances & Manufacturing Methods

14.1 Limits, Fits & Geometric Dimensioning & Tolerancing (GD&T) 14.2 Manufacturing Methods, Machinability, Heat Treatment & Assembly

15 Chapter 15: Supportive Knowledge: Codes, Computation, Testing & Corrosion

15.1 Engineering Codes & Standards 15.2 Computational Methods: FEA & Numerical Analysis 15.3 Instrumentation, Testing, Inspection & Quality 15.4 Chemical Processes: Corrosion, Oxidation & Embrittlement

6.1 High-Cycle Fatigue, S-N Curves & Marin Modifying Factors

Key Takeaways Explain This Topic AI

Fatigue failure progresses through three distinct physical stages: Stage I microcrack initiation along crystallographic shear planes, Stage II tensile opening mode crack propagation perpendicular to principal stresses (characterized by macroscopic beach marks and microscopic striations), and Stage III catastrophic fast fracture when the crack reaches critical length a c a_c a c ​ .

For steels with ultimate tensile strength S u t ≤ 200 kpsi S_{ut} \le 200\text{ kpsi} S u t ​ ≤ 200 kpsi ( 1400 MPa 1400\text{ MPa} 1400 MPa ), the uncorrected rotating-beam endurance limit is estimated as S e ′ ≈ 0.5 S u t S_e' \approx 0.5 S_{ut} S e ′ ​ ≈ 0.5 S u t ​ ; for higher tensile strengths, S e ′ S_e' S e ′ ​ plateaus at 100 kpsi 100\text{ kpsi} 100 kpsi ( 700 MPa 700\text{ MPa} 700 MPa ) due to heightened notch sensitivity to microscopic metallurgical inclusions.

Nonferrous metals (such as aluminum, magnesium, and copper alloys) do not exhibit a distinct horizontal endurance limit plateau; their fatigue strength S f S_f S f ​ continues to decline indefinitely with cycle count, requiring fatigue strength to be reported at a specified life (typically 5 × 10 8 5 \times 10^8 5 × 1 0 8 cycles).

The Marin endurance equation S e = k a k b k c k d k e k f S e ′ S_e = k_a k_b k_c k_d k_e k_f S_e' S e ​ = k a ​ k b ​ k c ​ k d ​ k e ​ k f ​ S e ′ ​ rigorously derates laboratory test specimens for real-world mechanical components based on surface finish ( k a k_a k a ​ ), physical size and stress gradient ( k b k_b k b ​ ), loading type ( k c k_c k c ​ ), operating temperature ( k d k_d k d ​ ), reliability requirements ( k e k_e k e ​ ), and environmental effects ( k f k_f k f ​ ).

The fatigue stress concentration factor K f = 1 + q ( K t − 1 ) K_f = 1 + q(K_t - 1) K f ​ = 1 + q ( K t ​ − 1 ) reflects the actual notch penalty, reduced from theoretical geometric stress concentration K t K_t K t ​ by notch sensitivity q q q , which depends on notch root radius ρ \rho ρ and the material's Neuber constant a \sqrt{a} a ​ .

Last updated: October 2026

6.1 High-Cycle Fatigue, S-N Curves & Marin Modifying Factors

Dynamic and cyclic loadings represent the primary cause of catastrophic structural and mechanical failures across engineering hardware. While static failure theories govern components subjected to invariant loads, dynamic failure can occur at stress levels drastically below the material's yield strength ( S y S_y S y ​ ) or ultimate tensile strength ( S u t S_{ut} S u t ​ ). Understanding high-cycle fatigue (HCF), stress-life ( S S S - N N N ) relationships, Marin modifying factors, and notch sensitivity is essential for machine design and failure prevention.

The Three Physical Stages of Fatigue Failure

Fatigue is a localized, progressive, and permanent structural damage process that occurs when materials are subjected to cyclic strains and stresses. Even when macroscopic stresses remain within the elastic regime, microscopic plastic deformation occurs at localized stress risers, slip planes, or material inhomogeneities. Fatigue failure unfolds across three distinct chronological stages: +-------------------------------------------------------------------------+

  • | Stage I: Microcrack Initiation |
  • | - Localized plastic shear along crystallographic slip bands (45° planes)|
  • | - Microscopic slip bands form extrusions and intrusions on free surface |
  • | - Typically consumes 80% to 90% of total life in smooth, pristine parts |
  • +------------------------------------+------------------------------------+
  • |
  • v
  • +------------------------------------+------------------------------------+
  • | Stage II: Stable Crack Propagation |
  • | - Crack turns 90° to propagate in Mode I (opening mode) |
  • | - Driven by alternating tensile principal stresses |
  • | - Produces macroscopic beach marks and microscopic striations |
  • +------------------------------------+------------------------------------+
  • |
  • v
  • +------------------------------------+------------------------------------+
  • | Stage III: Catastrophic Fast Fracture |
  • | - Remaining uncracked net ligament cross-section is overstressed |
  • | - Stress intensity reaches fracture toughness: K_I >= K_Ic |
  • | - Sudden, unstable ductile shear or brittle cleavage rupture |
  • +-------------------------------------------------------------------------+
  • 1. Stage I: Microcrack Initiation

Under cyclic shear stresses, dislocation movements cause slip along favorable crystallographic slip planes oriented at roughly 45° to the tensile stress axis. With repeated cycling, persistent slip bands (PSBs) emerge, producing microscopic valleys (intrusions) and peaks (extrusions) on the free surface. Intrusions act as severe stress micro-notches, concentrating cyclic strain until microcracks nucleate. In smooth, unnotched specimens operating in high-cycle fatigue, crack initiation consumes the vast majority (80% to 90%) of the component's total fatigue life.

2. Stage II: Stable Crack Propagation

Once a microcrack reaches a depth spanning several material grains (typically 0.1 to 0.2 mm 0.1\text{ to }0.2\text{ mm} 0.1 to 0.2 mm ), the stress field transitions from localized shear dominance to macroscopic tensile dominance. The crack changes direction, propagating perpendicular to the maximum alternating principal tensile stress in Mode I (opening mode). As the crack tip sharpens during tensile loading and blunts during compressive loading, it leaves distinct topographical features:

Microscopic Striations : Minute parallel ridges created during each individual cycle of loading. Striations are visible only under scanning electron microscopy (SEM) and directly map cycle-by-cycle crack advance.

Macroscopic Beach Marks (Progression Marks / Clamshell Marks) : Visible rings radiating outward from the initiation site, formed by changes in cyclic loading magnitude, machine stop-start intervals, or environmental oxidation during prolonged operation. Beach marks always point back toward the initiation site.

3. Stage III: Catastrophic Fast Fracture

As the stable crack reduces the uncracked cross-sectional area, the effective stress on the remaining ligament rises exponentially. When the crack reaches a critical flaw length a c a_c a c ​ such that the stress intensity factor equals or exceeds the material's plane-strain fracture toughness ( K I ≥ K I c K_I \ge K_{Ic} K I ​ ≥ K I c ​ ), the crack propagates unstably at high speed. The final failure surface exhibits ductile shear lips or brittle crystalline cleavage, representing an immediate, catastrophic rupture without warning.

The Rotating-Beam Test & Uncorrected Endurance Limit ( S e ′ S_e' S e ′ ​ )

Laboratory baseline fatigue properties are established using the standardized R.R. Moore rotating-beam test machine : Pure Bending Moment (No Shear Force) Fully Reversed Bending

  • ==================================== ======================
  • F/2 F/2 Stress Ratio: R = -1
  • | | Mean Stress: sigma_m = 0
  • +-----v---------------+-----+
  • Motor | =====[Specimen Neck]===== | Bearing Cycle Period: 1,800 rpm
  • +---------------------------+ Surface: Polished mirror

In this apparatus, a polished cylindrical specimen having a minimum neck diameter of d = 0.30 in d = 0.30\text{ in} d = 0.30 in ( 7.62 mm 7.62\text{ mm} 7.62 mm ) is supported in bearings and loaded with pure bending moments. As the motor rotates the specimen at high speed (typically 1 , 800 rpm 1,800\text{ rpm} 1 , 800 rpm ), every point on the neck surface undergoes fully reversed sinusoidal tension and compression ( R = σ min ⁡ / σ max ⁡ = − 1 R = \sigma_{\min}/\sigma_{\max} = -1 R = σ m i n ​ / σ m a x ​ = − 1 ) with zero mean stress ( σ m = 0 \sigma_m = 0 σ m ​ = 0 ).

Endurance Limit Estimation for Steels

When test results for polished carbon and alloy steels are plotted on semi-logarithmic or log-log axes ( % \% % of S u t S_{ut} S u t ​ vs cycles N N N ), the curve flattens into a horizontal plateau at approximately 10 6 10^6 1 0 6 cycles. This threshold stress is the uncorrected endurance limit ( S e ′ S_e' S e ′ ​ ), below which the specimen can endure an infinite number of load cycles without fracturing: S e ′ = { 0.50 S u t for S u t ≤ 200 kpsi ( 1400 MPa ) 100 kpsi ( 700 MPa ) for S u t > 200 kpsi ( 1400 MPa ) S_e' = \begin{cases}

  • 0.50 S_{ut} & \text{for } S_{ut} \le 200\text{ kpsi } (1400\text{ MPa}) \\
  • 100\text{ kpsi } (700\text{ MPa}) & \text{for } S_{ut} > 200\text{ kpsi } (1400\text{ MPa})

\end{cases} S e ′ ​ = { 0.50 S u t ​ 100 kpsi ( 700 MPa ) ​ for S u t ​ ≤ 200 kpsi ( 1400 MPa ) for S u t ​ > 200 kpsi ( 1400 MPa ) ​

Important

Why does S e ′ S_e' S e ′ ​ plateau at 100 kpsi 100\text{ kpsi} 100 kpsi ( 700 MPa 700\text{ MPa} 700 MPa )? As steel is heat-treated to ultra-high ultimate tensile strengths ( S u t > 200 kpsi S_{ut} > 200\text{ kpsi} S u t ​ > 200 kpsi ), its ductility and fracture toughness decrease drastically. The material becomes hyper-sensitive to microscopic non-metallic inclusions, micro-voids, and surface micro-imperfections. These internal defects act as pre-existing sharp cracks, suppressing the endurance limit below the theoretical 0.50 S u t 0.50 S_{ut} 0.50 S u t ​ value.

Nonferrous Alloys vs. Steels

Ferrous metals, titanium alloys, and certain polymers display a true endurance limit plateau. In contrast, nonferrous engineering alloys (including wrought and cast aluminum, magnesium, brass, and copper alloys) do not possess a true endurance limit . Their S S S - N N N curves continue to decrease continuously with increasing cycles. For nonferrous alloys, engineers must design for a finite service life using a fatigue strength ( S f , N S_{f,N} S f , N ​ ) defined at a designated cycle count—typically S f , 5 × 10 8 ≈ 0.30 to 0.40 S u t S_{f,5\times 10^8} \approx 0.30\text{ to }0.40 S_{ut} S f , 5 × 1 0 8 ​ ≈ 0.30 to 0.40 S u t ​ at N = 5 × 10 8 N = 5 \times 10^8 N = 5 × 1 0 8 cycles.

Finite-Life Fatigue Strength & Basquin's Equation

In many applications (e.g., aerospace frames, automotive suspension arms, pressure relief cycles), designing for infinite life results in excessive weight and cost. Instead, components are designed for a specified finite service life ( N N N cycles) in the high-cycle fatigue regime ( 10 3 ≤ N ≤ 10 6 10^3 \le N \le 10^6 1 0 3 ≤ N ≤ 1 0 6 cycles). Log(Stress) ^

  • S_ut +----------------------+
  • | Low-Cycle Fatigue |
  • | (Plastic Strain Dom) |
  • f * S_ut + - - - - - - - - - - - + - - - - - - - - - - - - - - - - - +
  • | \ High-Cycle Fatigue |
  • | \ (Basquin Power-Law Regime) |
  • S_e + - - - - - - - - - - - - - - - - - - - - - - - +===========+
  • | | Infinite |
  • | | Life Zone |
  • +-----------------------+-----------------------+-----------+--->
  • 10^3 10^6 Log(N)
  • Basquin's Power-Law Formulation

On a log-log coordinate grid, the high-cycle fatigue curve between 10 3 10^3 1 0 3 cycles and 10 6 10^6 1 0 6 cycles is idealized as a straight line described by Basquin's equation : S f = a N b S_f = a N^b S f ​ = a N b

where:

S f S_f S f ​ is the fatigue strength at N N N cycles.

a a a is the fatigue strength coefficient.

b b b is the fatigue strength exponent (Basquin's slope).

f f f is the fatigue strength fraction at 10 3 10^3 1 0 3 cycles ( S 10 3 = f S u t S_{10^3} = f S_{ut} S 1 0 3 ​ = f S u t ​ ).

For typical steels in bending, f f f ranges from 0.75 0.75 0.75 to 0.90 0.90 0.90 , commonly approximated as f = 0.90 f = 0.90 f = 0.90 for S u t ≤ 70 kpsi S_{ut} \le 70\text{ kpsi} S u t ​ ≤ 70 kpsi and decreasing toward f = 0.80 – 0.85 f = 0.80\text{--}0.85 f = 0.80 – 0.85 for high-strength steels.

At the two boundary conditions:

At N = 10 3 N = 10^3 N = 1 0 3 cycles: S f = f S u t = a ( 10 3 ) b S_f = f S_{ut} = a (10^3)^b S f ​ = f S u t ​ = a ( 1 0 3 ) b

At N = 10 6 N = 10^6 N = 1 0 6 cycles: S f = S e = a ( 10 6 ) b S_f = S_e = a (10^6)^b S f ​ = S e ​ = a ( 1 0 6 ) b

Solving these two simultaneous logarithmic equations yields the fundamental Basquin constants: a = ( f S u t ) 2 S e a = \frac{(f S_{ut})^2}{S_e} a = S e ​ ( f S u t ​ ) 2 ​ b = − 1 3 log ⁡ 10 ( f S u t S e ) b = -\frac{1}{3} \log_{10}\left(\frac{f S_{ut}}{S_e}\right) b = − 3 1 ​ lo g 10 ​ ( S e ​ f S u t ​ ​ )

Calculating Cycles to Failure

When a machine element is subjected to a completely reversed alternating stress amplitude σ rev \sigma_{\text{rev}} σ rev ​ that exceeds the endurance limit ( S e < σ rev < f S u t S_e < \sigma_{\text{rev}} < f S_{ut} S e ​ < σ rev ​ < f S u t ​ ), its predicted fatigue life N N N until failure is calculated by inverting Basquin's equation: N = ( σ rev a ) 1 / b N = \left(\frac{\sigma_{\text{rev}}}{a}\right)^{1/b} N = ( a σ rev ​ ​ ) 1/ b

Marin Endurance Modifying Factors ( S e = k a k b k c k d k e k f S e ′ S_e = k_a k_b k_c k_d k_e k_f S_e' S e ​ = k a ​ k b ​ k c ​ k d ​ k e ​ k f ​ S e ′ ​ )

The laboratory uncorrected endurance limit S e ′ S_e' S e ′ ​ applies strictly to mirror-polished, small ( 0.30 in 0.30\text{ in} 0.30 in ), unnotched specimens tested in room-temperature dry air under pure rotating bending. Real-world mechanical parts differ in surface texture, cross-sectional geometry, loading mode, operating temperature, and environmental exposure. Joseph Marin formulated an empirical modifying framework to derive the working endurance limit ( S e S_e S e ​ ): S e = k a k b k c k d k e k f S e ′ S_e = k_a k_b k_c k_d k_e k_f S_e' S e ​ = k a ​ k b ​ k c ​ k d ​ k e ​ k f ​ S e ′ ​

1. Surface Condition Factor ( k a k_a k a ​ )

Fatigue cracks almost invariably initiate at the outer free surface where alternating tensile stresses peak and surface micro-irregularities act as stress risers. The surface factor is computed using the power-law relation: k a = a S u t b k_a = a S_{ut}^b k a ​ = a S u t b ​

  • Surface Finish Factor a a a (kpsi) Factor a a a (MPa) Exponent b b b
  • Ground 1.34 1.34 1.34 1.58 1.58 1.58 − 0.085 -0.085 − 0.085
  • Machined or Cold-Drawn 2.70 2.70 2.70 4.51 4.51 4.51 − 0.265 -0.265 − 0.265
  • Hot-Rolled 14.4 14.4 14.4 57.7 57.7 57.7 − 0.718 -0.718 − 0.718
  • As-Forged 39.9 39.9 39.9 272.0 272.0 272.0 − 0.995 -0.995 − 0.995

Note: These are the widely used Shigley coefficients; other references and later editions publish somewhat different fits, so use the table given in the problem or reference handbook. High-strength steels suffer much more severe percentage reductions in k a k_a k a ​ under rough finishes than softer, ductile steels because of their elevated notch sensitivity.

2. Size Factor ( k b k_b k b ​ )

Larger components exhibit lower fatigue limits due to two mechanisms: (1) statistical volume effect (a larger volume of highly stressed material has a higher statistical probability of containing a critical flaw or inclusion), and (2) stress gradient effect (larger diameters experience shallower stress gradients, leaving a thicker sub-surface layer subjected to near-peak stresses).

For rotating cylindrical shafts in bending and torsion: k b = { ( d / 0.3 ) − 0.107 = 0.879 d − 0.107 for 0.11 in ≤ d ≤ 2.0 in 0.91 d − 0.157 for 2.0 in < d ≤ 10 in k_b = \begin{cases}

  • (d / 0.3)^{-0.107} = 0.879 d^{-0.107} & \text{for } 0.11\text{ in} \le d \le 2.0\text{ in} \\
  • 0.91 d^{-0.157} & \text{for } 2.0\text{ in} < d \le 10\text{ in}

\end{cases} k b ​ = { ( d /0.3 ) − 0.107 = 0.879 d − 0.107 0.91 d − 0.157 ​ for 0.11 in ≤ d ≤ 2.0 in for 2.0 in < d ≤ 10 in ​

Some references simply set k b = 1 k_b = 1 k b ​ = 1 for d ≤ 0.30 in d \le 0.30\text{ in} d ≤ 0.30 in ( 7.6 mm 7.6\text{ mm} 7.6 mm , the rotating-beam specimen size). In metric units ( d d d in mm): k b = { 1.24 d − 0.107 for 2.79 mm ≤ d ≤ 51 mm 1.51 d − 0.157 for 51 mm < d ≤ 254 mm k_b = \begin{cases}

  • 1.24 d^{-0.107} & \text{for } 2.79\text{ mm} \le d \le 51\text{ mm} \\
  • 1.51 d^{-0.157} & \text{for } 51\text{ mm} < d \le 254\text{ mm}
  • \end{cases} k b ​ = { 1.24 d − 0.107 1.51 d − 0.157 ​ for 2.79 mm ≤ d ≤ 51 mm for 51 mm < d ≤ 254 mm ​

For non-rotating bending or non-circular sections, an equivalent diameter d e d_e d e ​ is calculated by equating the volume of material stressed above 95% of maximum stress ( A 95 A_{95} A 95 ​ ) to that of a rotating round beam ( A 95 = 0.0766 d 2 A_{95} = 0.0766 d^2 A 95 ​ = 0.0766 d 2 ):

Rectangular section ( b × h b \times h b × h , bending about horizontal axis): d e = 0.808 b h d_e = 0.808 \sqrt{b h} d e ​ = 0.808 bh ​

Non-rotating round bar (diameter d d d , bending): d e = 0.370 d d_e = 0.370 d d e ​ = 0.370 d

Pure Axial Loading : In pure axial tension-compression, the stress is uniformly distributed across the entire cross-section (zero stress gradient). Therefore, by definition: k b = 1.0 (Pure Axial Loading) k_b = 1.0 \quad \text{(Pure Axial Loading)} k b ​ = 1.0 (Pure Axial Loading)

3. Loading Factor ( k c k_c k c ​ )

Accounts for the stress state and cross-sectional gradient compared to pure rotating bending ( k c = 1.0 k_c = 1.0 k c ​ = 1.0 ): k c = { 1.00 for Bending 0.85 for Pure Axial Loading 0.59 for Pure Torsion / Shear k_c = \begin{cases}

  • 1.00 & \text{for Bending} \\
  • 0.85 & \text{for Pure Axial Loading} \\
  • 0.59 & \text{for Pure Torsion / Shear}
  • \end{cases} k c ​ = ⎩ ⎨ ⎧ ​ 1.00 0.85 0.59 ​ for Bending for Pure Axial Loading for Pure Torsion / Shear ​

Note

The torsional factor k c = 0.59 k_c = 0.59 k c ​ = 0.59 aligns closely with the Distortion Energy (von Mises) failure criterion: 1 / 3 ≈ 0.577 1/\sqrt{3} \approx 0.577 1/ 3 ​ ≈ 0.577 . In pure torsion, S s e ≈ 0.59 S e S_{se} \approx 0.59 S_e S se ​ ≈ 0.59 S e ​ .

4. Temperature Factor ( k d k_d k d ​ )

At moderate operating temperatures ( T ≤ 450 ∘ F / 230 ∘ C T \le 450^\circ\text{F} / 230^\circ\text{C} T ≤ 45 0 ∘ F /23 0 ∘ C ), fatigue strength tracks tensile strength. At elevated temperatures ( T > 450 ∘ F T > 450^\circ\text{F} T > 45 0 ∘ F ), oxidation accelerates and thermal creep mechanisms interact with cyclic strain, degrading fatigue resistance: k d = S T S R T = 0.975 + 0.432 × 10 − 3 T − 0.115 × 10 − 5 T 2 + 0.104 × 10 − 8 T 3 − 0.595 × 10 − 12 T 4 k_d = \frac{S_T}{S_{RT}} = 0.975 + 0.432\times 10^{-3} T - 0.115\times 10^{-5} T^2 + 0.104\times 10^{-8} T^3 - 0.595\times 10^{-12} T^4 k d ​ = S RT ​ S T ​ ​ = 0.975 + 0.432 × 1 0 − 3 T − 0.115 × 1 0 − 5 T 2 + 0.104 × 1 0 − 8 T 3 − 0.595 × 1 0 − 12 T 4

(with T T T in ∘ F ^\circ\text{F} ∘ F ). For temperatures from 70 ∘ F 70^\circ\text{F} 7 0 ∘ F to 400 ∘ F 400^\circ\text{F} 40 0 ∘ F , k d ≈ 1.00 k_d \approx 1.00 k d ​ ≈ 1.00 .

5. Reliability Factor ( k e k_e k e ​ )

Standard fatigue endurance limits represent a 50 % 50\% 50% survival probability (the mean of experimental scatter, with typical coefficient of variation C v ≈ 0.08 C_v \approx 0.08 C v ​ ≈ 0.08 ). For mission-critical mechanical systems, higher reliability is enforced through k e = 1 − 0.08 z a k_e = 1 - 0.08 z_a k e ​ = 1 − 0.08 z a ​ :

  • Desired Reliability Standard Normal Deviate ( z a z_a z a ​ ) Reliability Factor ( k e k_e k e ​ )
  • 50% 0.000 0.000 0.000 1.000 1.000 1.000
  • 90% 1.282 1.282 1.282 0.897 0.897 0.897
  • 95% 1.645 1.645 1.645 0.868 0.868 0.868
  • 99% 2.326 2.326 2.326 0.814 0.814 0.814
  • 99.9% 3.090 3.090 3.090 0.753 0.753 0.753
  • 99.99% 3.719 3.719 3.719 0.702 0.702 0.702
  • 6. Miscellaneous Effects Factor ( k f k_f k f ​ )

All other operating and environmental factors are grouped into k f k_f k f ​ :

Residual Stresses : Compressive surface stresses introduced by shot peening, roller burnishing, or cold-working inhibit crack opening and can boost fatigue life significantly ( k f > 1.0 k_f > 1.0 k f ​ > 1.0 ). In contrast, tensile residual stresses from unannealed grinding or welding degrade life.

Corrosion Fatigue : In corrosive environments (e.g., saltwater), pitting acts as continuous sharp notch generation. The S S S - N N N curve loses its endurance limit entirely; k f k_f k f ​ can fall below 0.30 0.30 0.30 .

Electroplating : Hard chrome plating or nickel plating introduces high tensile residual stresses and hydrogen embrittlement, reducing the endurance limit by 20 % to 40 % 20\%\text{ to }40\% 20% to 40% ( k f ≈ 0.60 – 0.80 k_f \approx 0.60\text{--}0.80 k f ​ ≈ 0.60 – 0.80 ).

Fretting Corrosion : Microscopic oscillating motion between tightly clamped contact surfaces produces micro-galling and debris pits, drastically lowering fatigue strength ( k f ≈ 0.25 – 0.60 k_f \approx 0.25\text{--}0.60 k f ​ ≈ 0.25 – 0.60 ).

Fatigue Stress Concentration Factor ( K f K_f K f ​ ) & Notch Sensitivity ( q q q )

Geometric stress concentrations (fillets, keyways, transverse holes, retaining ring grooves) concentrate stress elastically by a factor K t = σ max ⁡ / σ 0 K_t = \sigma_{\max} / \sigma_0 K t ​ = σ m a x ​ / σ 0 ​ . However, under dynamic cyclic loading, materials do not experience the full geometric penalty K t K_t K t ​ . Instead, they exhibit a smaller effective fatigue stress concentration factor ( K f K_f K f ​ ): K f = Unnotched Endurance Limit Notched Endurance Limit = S e S e , notched K_f = \frac{\text{Unnotched Endurance Limit}}{\text{Notched Endurance Limit}} = \frac{S_e}{S_{e,\text{notched}}} K f ​ = Notched Endurance Limit Unnotched Endurance Limit ​ = S e , notched ​ S e ​ ​

Notch Sensitivity Index ( q q q )

The notch sensitivity q q q is defined as the fraction of the geometric penalty realized by the material: q = K f − 1 K t − 1 ⟺ K f = 1 + q ( K t − 1 ) q = \frac{K_f - 1}{K_t - 1} \iff K_f = 1 + q(K_t - 1) q = K t ​ − 1 K f ​ − 1 ​ ⟺ K f ​ = 1 + q ( K t ​ − 1 )

where 0 ≤ q ≤ 1 0 \le q \le 1 0 ≤ q ≤ 1 :

If q = 0 q = 0 q = 0 : K f = 1.0 K_f = 1.0 K f ​ = 1.0 (material is completely insensitive to the notch, typical of grey cast iron where internal graphite flakes dwarf external notches).

If q = 1 q = 1 q = 1 : K f = K t K_f = K_t K f ​ = K t ​ (material is fully sensitive to the notch, typical of ultra-high-strength brittle alloys).

Neuber's Constant Formulation

Notch sensitivity is quantified by Neuber's equation as a function of notch root radius r r r (or ρ \rho ρ ) and the Neuber material constant a \sqrt{a} a ​ : q = 1 1 + a r q = \frac{1}{1 + \frac{\sqrt{a}}{\sqrt{r}}} q = 1 + r ​ a ​ ​ 1 ​

For steels under bending or axial fatigue loading, Neuber's constant a \sqrt{a} a ​ (in in \sqrt{\text{in}} in ​ ) correlates directly with ultimate tensile strength: a = 0.246 − 3.08 × 10 − 3 S u t + 1.51 × 10 − 5 S u t 2 − 2.67 × 10 − 8 S u t 3 ( S u t in kpsi ) \sqrt{a} = 0.246 - 3.08\times 10^{-3} S_{ut} + 1.51\times 10^{-5} S_{ut}^2 - 2.67\times 10^{-8} S_{ut}^3 \quad (S_{ut} \text{ in kpsi}) a ​ = 0.246 − 3.08 × 1 0 − 3 S u t ​ + 1.51 × 1 0 − 5 S u t 2 ​ − 2.67 × 1 0 − 8 S u t 3 ​ ( S u t ​ in kpsi )

For torsional shear loading, the shear notch sensitivity q s q_s q s ​ and fatigue shear stress concentration factor K f s K_{fs} K f s ​ use the torsional Neuber fit a s = 0.190 − 2.51 × 10 − 3 S u t + 1.35 × 10 − 5 S u t 2 − 2.67 × 10 − 8 S u t 3 \sqrt{a_s} = 0.190 - 2.51\times 10^{-3} S_{ut} + 1.35\times 10^{-5} S_{ut}^2 - 2.67\times 10^{-8} S_{ut}^3 a s ​ ​ = 0.190 − 2.51 × 1 0 − 3 S u t ​ + 1.35 × 1 0 − 5 S u t 2 ​ − 2.67 × 1 0 − 8 S u t 3 ​ ( in \sqrt{\text{in}} in ​ , with S u t S_{ut} S u t ​ in kpsi): K f s = 1 + q s ( K t s − 1 ) K_{fs} = 1 + q_s(K_{ts} - 1) K f s ​ = 1 + q s ​ ( K t s ​ − 1 )

Warning

Never apply K f K_f K f ​ to both the material endurance limit and the applied stress simultaneously. Either divide the endurance limit by K f K_f K f ​ ( S e / K f S_e / K_f S e ​ / K f ​ ) OR multiply the nominal alternating stress by K f K_f K f ​ ( σ a = K f σ 0 , a \sigma_a = K_f \sigma_{0,a} σ a ​ = K f ​ σ 0 , a ​ ). Standard mechanical engineering practice applies K f K_f K f ​ to the applied nominal stress: σ = K f σ 0 \sigma = K_f \sigma_0 σ = K f ​ σ 0 ​ .

Summary Table: Marin Modifying Factors & Relationships

Factor Symbol Governing Equation / Primary Value Physical Significance

Surface Finish k a k_a k a ​ k a = a S u t b k_a = a S_{ut}^b k a ​ = a S u t b ​ Penalizes micro-roughness which accelerates Stage I crack initiation

Component Size k b k_b k b ​ 0.879 d − 0.107 0.879 d^{-0.107} 0.879 d − 0.107 ( 0.11 ≤ d ≤ 2 in 0.11 \le d \le 2\text{ in} 0.11 ≤ d ≤ 2 in ); k b = 1.0 k_b = 1.0 k b ​ = 1.0 for axial Accounts for statistical defect volume and stress gradient

Loading Type k c k_c k c ​ Bending: 1.00 1.00 1.00 ; Axial: 0.85 0.85 0.85 ; Torsion: 0.59 0.59 0.59 Normalizes to rotating-beam pure bending test state

Temperature k d k_d k d ​ S T / S R T S_T / S_{RT} S T ​ / S RT ​ (Unity for T ≤ 450 ∘ F T \le 450^\circ\text{F} T ≤ 45 0 ∘ F ) Captures loss of tensile capacity and creep-fatigue coupling

Reliability k e k_e k e ​ 50 % : 1.000 50\%: 1.000 50% : 1.000 ; 90 % : 0.897 90\%: 0.897 90% : 0.897 ; 99 % : 0.814 99\%: 0.814 99% : 0.814 ; 99.9 % : 0.753 99.9\%: 0.753 99.9% : 0.753 Shifts threshold from mean ( 50 % 50\% 50% ) to specified survival rate

Miscellaneous k f k_f k f ​ Residual stress, plating, corrosion ( 1.0 1.0 1.0 baseline) Environmental degradation, coatings, and shot-peening

Notch Sensitivity q q q q = 1 / ( 1 + a / r ) q = 1 / (1 + \sqrt{a}/\sqrt{r}) q = 1/ ( 1 + a ​ / r ​ ) Attenuates geometric K t K_t K t ​ to effective fatigue factor K f K_f K f ​

  • Realistic Worked Engineering Scenario: Transmission Shaft Step Fillet D = 1.875 in d = 1.50 in
  • +---------------------+ +---------------------+
  • | | | |
  • M <====== | +---r----+ | ======> M
  • (Reversed) | (Fillet: r = 0.150 in) | (Reversed)
  • | +---r----+ |
  • +---------------------+ +---------------------+
  • Problem Statement

A solid stepped drive shaft for a high-speed centrifugal pump is fabricated from cold-drawn AISI 1045 steel having properties:

Ultimate tensile strength: S u t = 91.0 kpsi S_{ut} = 91.0\text{ kpsi} S u t ​ = 91.0 kpsi ( 627 MPa 627\text{ MPa} 627 MPa )

Yield strength: S y = 77.0 kpsi S_y = 77.0\text{ kpsi} S y ​ = 77.0 kpsi ( 531 MPa 531\text{ MPa} 531 MPa )

Geometric and operational parameters:

  • Major diameter: D = 1.875 in D = 1.875\text{ in} D = 1.875 in
  • Minor diameter: d = 1.500 in d = 1.500\text{ in} d = 1.500 in
  • Shoulder fillet radius: r = 0.150 in r = 0.150\text{ in} r = 0.150 in
  • Theoretical stress concentration factor in bending: K t = 1.68 K_t = 1.68 K t ​ = 1.68

Surface finish: Machined ( a = 2.70 a = 2.70 a = 2.70 , b = − 0.265 b = -0.265 b = − 0.265 for S u t S_{ut} S u t ​ in kpsi)

  • Operating environment: Ambient temperature ( 70 ∘ F 70^\circ\text{F} 7 0 ∘ F ), dry, no corrosive agents
  • Target reliability: 99 % 99\% 99% ( k e = 0.814 k_e = 0.814 k e ​ = 0.814 )

Applied cyclic load: Completely reversed bending moment M = 3 , 500 lbf ⋅ in M = 3,500\text{ lbf}\cdot\text{in} M = 3 , 500 lbf ⋅ in ( R = − 1 R = -1 R = − 1 )

Calculate:

The uncorrected endurance limit S e ′ S_e' S e ′ ​ and fully modified endurance limit S e S_e S e ​ .

The fatigue notch sensitivity q q q and fatigue stress concentration factor K f K_f K f ​ .

The peak alternating bending stress σ a \sigma_a σ a ​ and the factor of safety n f n_f n f ​ for infinite life.

The predicted fatigue life N N N (cycles) if an overload moment of M over = 6 , 500 lbf ⋅ in M_{\text{over}} = 6,500\text{ lbf}\cdot\text{in} M over ​ = 6 , 500 lbf ⋅ in is applied (using f = 0.875 f = 0.875 f = 0.875 ).

  • Step-by-Step Mathematical Solution
  • Step 1: Uncorrected Endurance Limit ( S e ′ S_e' S e ′ ​ )

Because S u t = 91.0 kpsi ≤ 200 kpsi S_{ut} = 91.0\text{ kpsi} \le 200\text{ kpsi} S u t ​ = 91.0 kpsi ≤ 200 kpsi : S e ′ = 0.50 S u t = 0.50 × 91.0 kpsi = 45.50 kpsi S_e' = 0.50 S_{ut} = 0.50 \times 91.0\text{ kpsi} = 45.50\text{ kpsi} S e ′ ​ = 0.50 S u t ​ = 0.50 × 91.0 kpsi = 45.50 kpsi

Step 2: Marin Endurance Modifying Factors

Surface factor ( k a k_a k a ​ ) : k a = a S u t b = 2.70 × ( 91.0 ) − 0.265 = 2.70 × 0.30259 = 0.8170 ≈ 0.817 k_a = a S_{ut}^b = 2.70 \times (91.0)^{-0.265} = 2.70 \times 0.30259 = 0.8170 \approx 0.817 k a ​ = a S u t b ​ = 2.70 × ( 91.0 ) − 0.265 = 2.70 × 0.30259 = 0.8170 ≈ 0.817

Size factor ( k b k_b k b ​ ) :

For rotating bending with d = 1.50 in d = 1.50\text{ in} d = 1.50 in ( 0.11 ≤ d ≤ 2.0 in 0.11 \le d \le 2.0\text{ in} 0.11 ≤ d ≤ 2.0 in ): k b = 0.879 d − 0.107 = 0.879 × ( 1.50 ) − 0.107 = 0.879 × 0.9575 = 0.842 k_b = 0.879 d^{-0.107} = 0.879 \times (1.50)^{-0.107} = 0.879 \times 0.9575 = 0.842 k b ​ = 0.879 d − 0.107 = 0.879 × ( 1.50 ) − 0.107 = 0.879 × 0.9575 = 0.842

(Equivalently, ( d / 0.3 ) − 0.107 = 5 − 0.107 = 0.842 (d/0.3)^{-0.107} = 5^{-0.107} = 0.842 ( d /0.3 ) − 0.107 = 5 − 0.107 = 0.842 .)

Load factor ( k c k_c k c ​ ) :

For pure bending loading, k c = 1.00 k_c = 1.00 k c ​ = 1.00 .

Temperature factor ( k d k_d k d ​ ) :

At 70 ∘ F 70^\circ\text{F} 7 0 ∘ F , k d = 1.00 k_d = 1.00 k d ​ = 1.00 .

Reliability factor ( k e k_e k e ​ ) :

For 99 % 99\% 99% reliability, k e = 0.814 k_e = 0.814 k e ​ = 0.814 .

Miscellaneous factor ( k f k_f k f ​ ) :

Standard baseline environment, k f = 1.00 k_f = 1.00 k f ​ = 1.00 .

Compute fully corrected endurance limit S e S_e S e ​ : S e = k a k b k c k d k e k f S e ′ = ( 0.817 ) × ( 0.842 ) × ( 1.00 ) × ( 1.00 ) × ( 0.814 ) × ( 1.00 ) × 45.50 kpsi S_e = k_a k_b k_c k_d k_e k_f S_e' = (0.817) \times (0.842) \times (1.00) \times (1.00) \times (0.814) \times (1.00) \times 45.50\text{ kpsi} S e ​ = k a ​ k b ​ k c ​ k d ​ k e ​ k f ​ S e ′ ​ = ( 0.817 ) × ( 0.842 ) × ( 1.00 ) × ( 1.00 ) × ( 0.814 ) × ( 1.00 ) × 45.50 kpsi S e = 0.5600 × 45.50 kpsi = 25.48 kpsi S_e = 0.5600 \times 45.50\text{ kpsi} = 25.48\text{ kpsi} S e ​ = 0.5600 × 45.50 kpsi = 25.48 kpsi

Step 3: Notch Sensitivity q q q and Fatigue Concentration K f K_f K f ​

Determine Neuber constant a \sqrt{a} a ​ for S u t = 91 kpsi S_{ut} = 91\text{ kpsi} S u t ​ = 91 kpsi (bending): a = 0.246 − 3.08 × 10 − 3 ( 91 ) + 1.51 × 10 − 5 ( 91 ) 2 − 2.67 × 10 − 8 ( 91 ) 3 = 0.246 − 0.2803 + 0.1250 − 0.0201 = 0.0706 in \sqrt{a} = 0.246 - 3.08\times 10^{-3}(91) + 1.51\times 10^{-5}(91)^2 - 2.67\times 10^{-8}(91)^3 = 0.246 - 0.2803 + 0.1250 - 0.0201 = 0.0706\,\sqrt{\text{in}} a ​ = 0.246 − 3.08 × 1 0 − 3 ( 91 ) + 1.51 × 1 0 − 5 ( 91 ) 2 − 2.67 × 1 0 − 8 ( 91 ) 3 = 0.246 − 0.2803 + 0.1250 − 0.0201 = 0.0706 in ​

Compute notch sensitivity q q q with fillet radius r = 0.150 in r = 0.150\text{ in} r = 0.150 in : q = 1 1 + a r = 1 1 + 0.0706 0.150 = 1 1 + 0.0706 0.3873 = 1 1 + 0.1824 = 0.8457 ≈ 0.846 q = \frac{1}{1 + \frac{\sqrt{a}}{\sqrt{r}}} = \frac{1}{1 + \frac{0.0706}{\sqrt{0.150}}} = \frac{1}{1 + \frac{0.0706}{0.3873}} = \frac{1}{1 + 0.1824} = 0.8457 \approx 0.846 q = 1 + r ​ a ​ ​ 1 ​ = 1 + 0.150 ​ 0.0706 ​ 1 ​ = 1 + 0.3873 0.0706 ​ 1 ​ = 1 + 0.1824 1 ​ = 0.8457 ≈ 0.846

Compute fatigue stress concentration factor K f K_f K f ​ : K f = 1 + q ( K t − 1 ) = 1 + 0.846 ( 1.68 − 1 ) = 1 + 0.846 ( 0.68 ) = 1 + 0.575 = 1.575 K_f = 1 + q(K_t - 1) = 1 + 0.846(1.68 - 1) = 1 + 0.846(0.68) = 1 + 0.575 = 1.575 K f ​ = 1 + q ( K t ​ − 1 ) = 1 + 0.846 ( 1.68 − 1 ) = 1 + 0.846 ( 0.68 ) = 1 + 0.575 = 1.575

Step 4: Nominal Stress, Peak Stress & Factor of Safety

Elastic section modulus for solid circular cross-section at minor diameter d = 1.50 in d = 1.50\text{ in} d = 1.50 in : Z = π d 3 32 = π ( 1.50 ) 3 32 = 3.375 π 32 = 0.33134 in 3 Z = \frac{\pi d^3}{32} = \frac{\pi (1.50)^3}{32} = \frac{3.375 \pi}{32} = 0.33134\text{ in}^3 Z = 32 π d 3 ​ = 32 π ( 1.50 ) 3 ​ = 32 3.375 π ​ = 0.33134 in 3

Nominal alternating bending stress σ 0 \sigma_0 σ 0 ​ : σ 0 = M Z = 3,500 lbf ⋅ in 0.33134 in 3 = 10,563 psi = 10.56 kpsi \sigma_0 = \frac{M}{Z} = \frac{3{,}500\text{ lbf}\cdot\text{in}}{0.33134\text{ in}^3} = 10{,}563\text{ psi} = 10.56\text{ kpsi} σ 0 ​ = Z M ​ = 0.33134 in 3 3 , 500 lbf ⋅ in ​ = 10 , 563 psi = 10.56 kpsi

Actual peak alternating stress σ a \sigma_a σ a ​ applying K f K_f K f ​ : σ a = K f σ 0 = 1.575 × 10.563 kpsi = 16.64 kpsi \sigma_a = K_f \sigma_0 = 1.575 \times 10.563\text{ kpsi} = 16.64\text{ kpsi} σ a ​ = K f ​ σ 0 ​ = 1.575 × 10.563 kpsi = 16.64 kpsi

Factor of safety for infinite life ( n f n_f n f ​ ): n f = S e σ a = 25.48 kpsi 16.64 kpsi = 1.53 n_f = \frac{S_e}{\sigma_a} = \frac{25.48\text{ kpsi}}{16.64\text{ kpsi}} = 1.53 n f ​ = σ a ​ S e ​ ​ = 16.64 kpsi 25.48 kpsi ​ = 1.53

Because n f = 1.53 > 1.0 n_f = 1.53 > 1.0 n f ​ = 1.53 > 1.0 , the shaft operates safely in the infinite-life regime under the 3,500 lbf ⋅ in 3{,}500\text{ lbf}\cdot\text{in} 3 , 500 lbf ⋅ in moment.

Step 5: Finite-Life Evaluation Under Overload Moment

When the bending moment increases to M over = 6,500 lbf ⋅ in M_{\text{over}} = 6{,}500\text{ lbf}\cdot\text{in} M over ​ = 6 , 500 lbf ⋅ in : σ 0 , over = 6,500 0.33134 = 19,617 psi = 19.62 kpsi \sigma_{0,\text{over}} = \frac{6{,}500}{0.33134} = 19{,}617\text{ psi} = 19.62\text{ kpsi} σ 0 , over ​ = 0.33134 6 , 500 ​ = 19 , 617 psi = 19.62 kpsi σ a , over = K f σ 0 , over = 1.575 × 19.617 kpsi = 30.90 kpsi \sigma_{a,\text{over}} = K_f \sigma_{0,\text{over}} = 1.575 \times 19.617\text{ kpsi} = 30.90\text{ kpsi} σ a , over ​ = K f ​ σ 0 , over ​ = 1.575 × 19.617 kpsi = 30.90 kpsi

Because σ a , over = 30.90 kpsi > S e = 25.48 kpsi \sigma_{a,\text{over}} = 30.90\text{ kpsi} > S_e = 25.48\text{ kpsi} σ a , over ​ = 30.90 kpsi > S e ​ = 25.48 kpsi , the shaft has a finite fatigue life.

Compute Basquin constants ( f = 0.875 f = 0.875 f = 0.875 ): f S u t = 0.875 × 91.0 kpsi = 79.625 kpsi f S_{ut} = 0.875 \times 91.0\text{ kpsi} = 79.625\text{ kpsi} f S u t ​ = 0.875 × 91.0 kpsi = 79.625 kpsi a = ( f S u t ) 2 S e = ( 79.625 ) 2 25.48 = 6340.14 25.48 = 248.83 kpsi a = \frac{(f S_{ut})^2}{S_e} = \frac{(79.625)^2}{25.48} = \frac{6340.14}{25.48} = 248.83\text{ kpsi} a = S e ​ ( f S u t ​ ) 2 ​ = 25.48 ( 79.625 ) 2 ​ = 25.48 6340.14 ​ = 248.83 kpsi b = − 1 3 log ⁡ 10 ( f S u t S e ) = − 1 3 log ⁡ 10 ( 79.625 25.48 ) = − 1 3 log ⁡ 10 ( 3.1250 ) = − 1 3 ( 0.49485 ) = − 0.16495 b = -\frac{1}{3} \log_{10}\left(\frac{f S_{ut}}{S_e}\right) = -\frac{1}{3} \log_{10}\left(\frac{79.625}{25.48}\right) = -\frac{1}{3} \log_{10}(3.1250) = -\frac{1}{3}(0.49485) = -0.16495 b = − 3 1 ​ lo g 10 ​ ( S e ​ f S u t ​ ​ ) = − 3 1 ​ lo g 10 ​ ( 25.48 79.625 ​ ) = − 3 1 ​ lo g 10 ​ ( 3.1250 ) = − 3 1 ​ ( 0.49485 ) = − 0.16495

Calculate cycles to failure N N N : N = ( σ a , over a ) 1 / b = ( 30.90 248.83 ) − 1 / 0.16495 = ( 0.12418 ) − 6.0624 ≈ 311,000 cycles N = \left(\frac{\sigma_{a,\text{over}}}{a}\right)^{1/b} = \left(\frac{30.90}{248.83}\right)^{-1/0.16495} = (0.12418)^{-6.0624} \approx 311{,}000\text{ cycles} N = ( a σ a , over ​ ​ ) 1/ b = ( 248.83 30.90 ​ ) − 1/0.16495 = ( 0.12418 ) − 6.0624 ≈ 311 , 000 cycles

The stepped shaft is expected to survive approximately 3.1 × 10 5 3.1 \times 10^5 3.1 × 1 0 5 cycles at the overload moment before fatigue fracture.