Study guide
2.1 Stress-Strain Relationships & Fundamental Mechanical Properties
PE Mechanical: Machine Design and Materials Exam
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Basic Engineering Practice: Drawings, Economics & Design Methodology
1.1 Engineering Terms, Symbols, Drawing Interpretation & Conventions 1.2 Project Management & Engineering Economics 1.3 Design Methodology, Risk Assessment & Safety
2 Chapter 2: Physical & Mechanical Properties of Engineering Materials
2.1 Stress-Strain Relationships & Fundamental Mechanical Properties 2.2 Physical Properties, Temperature Effects, Hardness, Impact Toughness & Creep
3 Chapter 3: Mechanics of Materials: Fundamental Loadings & Deflections
3.1 Axial Loading, Normal Stress & Statically Indeterminate Members 3.2 Direct Shear, Bearing & Transverse Shear in Beams 3.3 Torsion of Shafts, Power Transmission & Thin-Walled Tubes 3.4 Beam Bending Stresses & Deflection Analysis
4 Chapter 4: Mechanics of Materials: Stability, Multiaxial Stress & Thermal Effects
4.1 Column Buckling & Elastic/Inelastic Instability 4.2 Combined Loading, Principal Stresses & Mohr's Circle 4.3 Thermal Stresses & Interference Stresses
5 Chapter 5: Failure Theories: Static Yielding & Fracture Mechanics
5.1 Static Failure Theories for Ductile Materials: von Mises & Tresca 5.2 Static Failure Theories for Brittle Materials & Fracture Mechanics
6 Chapter 6: Fatigue Analysis & Dynamic Failure
6.1 High-Cycle Fatigue, S-N Curves & Marin Modifying Factors 6.2 Fluctuating Stresses, Failure Criteria & Cumulative Damage
7 Chapter 7: Mechanical Attachments: Fasteners & Bolted Joints
7.1 Threaded Fasteners, Proof Strength & Preload Mechanics 7.2 Bolted Joint Stiffness, External Loading & Separation 7.3 Non-Threaded Fasteners: Keys, Pins, Clevises, Retaining Rings, Rivets, Lugs & Anchors
8 Chapter 8: Mechanical Attachments: Permanent Joints & Bonding
8.1 Welded Joints & Weld Group Stress Analysis 8.2 Brazing, Soldering & Structural Adhesive Bonding
9 Chapter 9: Power Transmission: Shafts & Gearing
9.1 Transmission Shaft Design, Critical Speeds & Deflection 9.2 Spur Gears: Geometry, Kinematics & AGMA Stress Equations 9.3 Helical, Bevel & Worm Gearing
10 Chapter 10: Power Transmission: Bearings, Flexible Drives, Friction Devices & Prime Movers
10.1 Rolling-Element Bearings & L10 Life Calculations 10.2 Hydrodynamic Journal Bearings & Lubrication Regimes 10.3 Belts, Roller Chains & Flexible Drives 10.4 Clutches, Brakes & Power Screws 10.5 Electric Motors, Engines & Flywheels
11 Chapter 11: Mechanical Components: Pressure Vessels & Structural Systems
11.1 Pressure Vessels & Piping: Thin and Thick Walls, ASME VIII and B31 11.2 Mechanical Springs: Helical, Belleville & Leaf Springs 11.3 Structural Trusses, Rigid Frames & Energy Methods
12 Chapter 12: Mechanical Dynamics, Vibrations & Fluid Power
12.1 Single-Degree-of-Freedom Vibrations & Resonance 12.2 Vibration Isolation, Multi-DOF Systems & Transmissibility 12.3 Fluid Power Systems: Hydraulics & Pneumatics
13 Chapter 13: Kinematics, Mechatronics & Control Systems
13.1 Mechanism Kinematics, Linkages, Cams & Simple Machines 13.2 Basic Mechatronics, Sensors & Closed-Loop Controls
14 Chapter 14: Supportive Knowledge: Fits, Tolerances & Manufacturing Methods
14.1 Limits, Fits & Geometric Dimensioning & Tolerancing (GD&T) 14.2 Manufacturing Methods, Machinability, Heat Treatment & Assembly
15 Chapter 15: Supportive Knowledge: Codes, Computation, Testing & Corrosion
15.1 Engineering Codes & Standards 15.2 Computational Methods: FEA & Numerical Analysis 15.3 Instrumentation, Testing, Inspection & Quality 15.4 Chemical Processes: Corrosion, Oxidation & Embrittlement
2.1 Stress-Strain Relationships & Fundamental Mechanical Properties
Key Takeaways Explain This Topic AI
Engineering stress and strain ( σ = P / A 0 , ϵ = Δ L / L 0 \sigma = P/A_0, \epsilon = \Delta L/L_0 σ = P / A 0 , ϵ = Δ L / L 0 ) reference initial dimensions, whereas true stress and strain ( σ T = σ ( 1 + ϵ ) , ϵ T = ln ( 1 + ϵ ) \sigma_T = \sigma(1+\epsilon), \epsilon_T = \ln(1+\epsilon) σ T = σ ( 1 + ϵ ) , ϵ T = ln ( 1 + ϵ ) ) account for instantaneous area up to localized necking.
For isotropic linear elastic materials, the shear modulus G G G , elastic modulus E E E , and Poisson's ratio ν \nu ν are coupled by G = E 2 ( 1 + ν ) G = \frac{E}{2(1+\nu)} G = 2 ( 1 + ν ) E , reducing the number of independent elastic constants to two.
The 0.2% offset yield strength ( S y S_y S y ) establishes the boundary of macroscopic plastic deformation for materials without a distinct yield plateau, such as aluminum alloys and high-strength steels.
Modulus of resilience ( U r = S y 2 2 E U_r = \frac{S_y^2}{2E} U r = 2 E S y 2 ) quantifies elastic energy storage capacity per unit volume, serving as the primary figure of merit for mechanical springs and compliant flexures.
Heat treatment and cold work alter yield and tensile strengths by hundreds of percent but leave Young's modulus E E E virtually unchanged because E E E is dictated strictly by interatomic bond stiffness.
Last updated: October 2026
2.1 Stress-Strain Relationships & Fundamental Mechanical Properties
Quick Summary: Uniaxial tensile testing provides the empirical foundation for machine design by quantifying how materials deform under static mechanical loads. This section establishes the distinction between engineering and true stress-strain metrics, details isotropic elastic constitutive relations ( E E E , G G G , ν \nu ν ), defines critical transition boundaries from proportional limit to fracture, evaluates energy absorption criteria (resilience and toughness), and compares baseline mechanical properties across dominant structural engineering alloys.
1. Uniaxial Tensile Testing & Stress-Strain Foundations
The standardized uniaxial tensile test (ASTM E8 / E8M) is the foundational experimental method for determining the static mechanical properties of engineering materials. A standardized specimen with initial gage length L 0 L_0 L 0 and initial cross-sectional area A 0 A_0 A 0 is mounted in crossheads and subjected to quasi-static axial elongation until fracture.
Engineering Stress and Engineering Strain
In standard machine design practice, tensile test data are conventionally recorded in terms of engineering stress (nominal stress, σ \sigma σ ) and engineering strain (nominal strain, ϵ \epsilon ϵ ):
σ = P A 0 \sigma = \frac{P}{A_0} σ = A 0 P
ϵ = Δ L L 0 = L − L 0 L 0 \epsilon = \frac{\Delta L}{L_0} = \frac{L - L_0}{L_0} ϵ = L 0 Δ L = L 0 L − L 0
where P P P is the instantaneous applied tensile force, L L L is the instantaneous gage length, and Δ L \Delta L Δ L is the total axial elongation. Because engineering stress and strain are normalized against fixed initial specimen dimensions ( A 0 A_0 A 0 and L 0 L_0 L 0 ), they provide convenient values for component design where dimensional changes prior to yielding are negligible ( < 0.2 % < 0.2\% < 0.2% ).
True Stress and True Strain
When analyzing large plastic deformation, metal forming processes, or ductile fracture mechanics, engineering measures become physically misleading because the cross-sectional area changes continuously. True stress (flow stress, σ T \sigma_T σ T ) and true strain (logarithmic or natural strain, ϵ T \epsilon_T ϵ T ) are defined using the instantaneous load and instantaneous dimensions:
σ T = P A \sigma_T = \frac{P}{A} σ T = A P
ϵ T = ∫ L 0 L d L L = ln ( L L 0 ) \epsilon_T = \int_{L_0}^{L} \frac{dL}{L} = \ln\left(\frac{L}{L_0}\right) ϵ T = ∫ L 0 L L d L = ln ( L 0 L )
where A A A is the instantaneous load-bearing cross-sectional area.
Conversion Relationships Before Necking
During uniform plastic deformation prior to the onset of localized necking, the volume of the metallic specimen remains essentially constant because plastic deformation occurs via dislocation glide without changing crystal density ( V = A L = A 0 L 0 V = A L = A_0 L_0 V = A L = A 0 L 0 ). Under this constant volume condition:
A 0 A = L L 0 = L 0 + Δ L L 0 = 1 + ϵ \frac{A_0}{A} = \frac{L}{L_0} = \frac{L_0 + \Delta L}{L_0} = 1 + \epsilon A A 0 = L 0 L = L 0 L 0 + Δ L = 1 + ϵ
Substituting this geometric equivalence yields the direct conversion formulas between engineering and true parameters:
σ T = P A = P A 0 ( A 0 A ) = σ ( 1 + ϵ ) \sigma_T = \frac{P}{A} = \frac{P}{A_0} \left(\frac{A_0}{A}\right) = \sigma (1 + \epsilon) σ T = A P = A 0 P ( A A 0 ) = σ ( 1 + ϵ )
ϵ T = ln ( L L 0 ) = ln ( 1 + ϵ ) \epsilon_T = \ln\left(\frac{L}{L_0}\right) = \ln(1 + \epsilon) ϵ T = ln ( L 0 L ) = ln ( 1 + ϵ )
Important Examination Note: These conversion equations are strictly valid only up to the ultimate tensile strength ( S u t S_{ut} S u t ) . At S u t S_{ut} S u t , plastic instability initiates localized necking, non-uniform triaxial stress states develop within the neck, and volume constancy over the original gage length no longer describes local behavior. Beyond S u t S_{ut} S u t , true stress must be determined by directly measuring the minimum neck cross-sectional area: σ T = P / A neck \sigma_T = P / A_{\text{neck}} σ T = P / A neck .
Flow Stress & The Hollomon Power Law
In the uniform plastic strain regime between yielding and necking, the true stress-strain behavior of most ductile polycrystalline metals is modeled by the Hollomon equation (power-law strain hardening):
σ T = K ϵ T n \sigma_T = K \epsilon_T^n σ T = K ϵ T n
where K K K is the strength coefficient (true stress at ϵ T = 1.0 \epsilon_T = 1.0 ϵ T = 1.0 ) and n n n is the strain-hardening exponent (typically 0.10 ≤ n ≤ 0.50 0.10 \le n \le 0.50 0.10 ≤ n ≤ 0.50 for structural metals). By applying the Considère criterion for necking instability ( d σ T / d ϵ T = σ T d\sigma_T / d\epsilon_T = \sigma_T d σ T / d ϵ T = σ T ), it can be shown that necking begins precisely when the true strain equals the strain-hardening exponent: ϵ T , neck = n \epsilon_{T,\text{neck}} = n ϵ T , neck = n .
2. Elastic Behavior, Hooke's Law & Isotropic Elastic Moduli
Within the linear elastic regime, deformation is completely reversible: atomic bonds are stretched without dislocation motion, and upon load removal, the specimen returns exactly to its original dimensions.
One-Dimensional Hooke's Law
Linear elasticity in uniaxial loading is governed by Hooke's Law:
σ = E ϵ \sigma = E \epsilon σ = E ϵ
where E E E is the Modulus of Elasticity (Young's Modulus). Young's modulus represents the fundamental stiffness of the material's atomic bonds. Because E E E is governed by interatomic potentials:
Thermal treatments (e.g., quenching, tempering, annealing) and mechanical cold work change yield and tensile strengths significantly, but have virtually no effect on E E E .
For carbon and low-alloy steels, E ≈ 200 – 207 GPa E \approx 200\text{--}207\text{ GPa} E ≈ 200 – 207 GPa ( 29 – 30 Mpsi 29\text{--}30\text{ Mpsi} 29 – 30 Mpsi ); austenitic stainless steels are slightly lower, about 193 GPa 193\text{ GPa} 193 GPa ( 28 Mpsi 28\text{ Mpsi} 28 Mpsi ).
For aluminum alloys, E ≈ 69 – 72 GPa E \approx 69\text{--}72\text{ GPa} E ≈ 69 – 72 GPa ( 10.0 – 10.4 Mpsi 10.0\text{--}10.4\text{ Mpsi} 10.0 – 10.4 Mpsi ).
For titanium alloys, E ≈ 110 – 114 GPa E \approx 110\text{--}114\text{ GPa} E ≈ 110 – 114 GPa ( 16.0 – 16.5 Mpsi 16.0\text{--}16.5\text{ Mpsi} 16.0 – 16.5 Mpsi ).
Poisson's Ratio
When an axial tensile stress induces positive longitudinal strain ( ϵ x > 0 \epsilon_x > 0 ϵ x > 0 ), the cross-section undergoes simultaneous transverse contraction ( ϵ y = ϵ z < 0 \epsilon_y = \epsilon_z < 0 ϵ y = ϵ z < 0 ). Poisson's ratio ( ν \nu ν ) is defined as the negative ratio of lateral strain to longitudinal axial strain:
ν = − ϵ lateral ϵ axial = − ϵ y ϵ x = − ϵ z ϵ x \nu = -\frac{\epsilon_{\text{lateral}}}{\epsilon_{\text{axial}}} = -\frac{\epsilon_y}{\epsilon_x} = -\frac{\epsilon_z}{\epsilon_x} ν = − ϵ axial ϵ lateral = − ϵ x ϵ y = − ϵ x ϵ z
For theoretical isotropic elastic solids, thermodynamic stability requires − 1.0 < ν < 0.50 -1.0 < \nu < 0.50 − 1.0 < ν < 0.50 . For structural engineering metals, ν \nu ν typically ranges from 0.25 0.25 0.25 to 0.35 0.35 0.35 (structural steels ≈ 0.28 – 0.30 \approx 0.28\text{--}0.30 ≈ 0.28 – 0.30 , aluminum alloys ≈ 0.33 \approx 0.33 ≈ 0.33 , titanium ≈ 0.31 \approx 0.31 ≈ 0.31 , and gray cast iron ≈ 0.21 – 0.26 \approx 0.21\text{--}0.26 ≈ 0.21 – 0.26 ). Perfectly incompressible materials deforming at constant volume (such as rubber or metals under fully plastic flow) exhibit ν = 0.50 \nu = 0.50 ν = 0.50 .
Shear Modulus & Constitutive Coupling
Under pure torsional or transverse shear loading, shear stress ( τ \tau τ ) relates to engineering shear strain ( γ \gamma γ ) through the Shear Modulus ( G G G , also known as the Modulus of Rigidity):
τ = G γ \tau = G \gamma τ = G γ
For an isotropic material (whose physical properties are identical in all directions), directional symmetry dictates that normal and shear behaviors are coupled. The three primary elastic constants are interrelated by:
G = E 2 ( 1 + ν ) G = \frac{E}{2(1 + \nu)} G = 2 ( 1 + ν ) E
Similarly, the Bulk Modulus ( K K K ), which governs resistance to uniform hydrostatic compression ( p = − K Δ V / V 0 p = -K \Delta V / V_0 p = − K Δ V / V 0 ), is expressed as:
K = E 3 ( 1 − 2 ν ) K = \frac{E}{3(1 - 2\nu)} K = 3 ( 1 − 2 ν ) E
Because of these constitutive relationships, an isotropic linear elastic material requires only two independent elastic constants (e.g., E E E and ν \nu ν ) to completely define its three-dimensional elastic compliance matrix.
Isotropic vs. Anisotropic Material Behavior
Isotropic Materials: Randomly oriented equiaxed polycrystalline grains produce uniform mechanical response in every direction. Most cast, forged, and normalized structural metals behave isotropically on the macroscopic scale (2 independent elastic constants).
Orthotropic Materials: Possess three mutually orthogonal planes of material symmetry. Examples include unidirectional fiber-reinforced composites, rolled sheet metals exhibiting planar anisotropy (different rolling vs. transverse properties), and wood. Orthotropic materials require 9 independent elastic constants ( E x , E y , E z , G x y , G y z , G z x , ν x y , ν y z , ν z x E_x, E_y, E_z, G_{xy}, G_{yz}, G_{zx}, \nu_{xy}, \nu_{yz}, \nu_{zx} E x , E y , E z , G x y , G yz , G z x , ν x y , ν yz , ν z x ).
Anisotropic (Triclinic) Materials: Exhibit completely direction-dependent properties with no planes of symmetry, requiring 21 independent elastic stiffness coefficients in the generalized Hooke's law tensor ( σ i j = C i j k l ϵ k l \sigma_{ij} = C_{ijkl} \epsilon_{kl} σ ij = C ijk l ϵ k l ).
3. Transition Boundaries on the Engineering Stress-Strain Curve
A complete engineering stress-strain curve for a ductile structural alloy reveals distinct mechanical transition thresholds: Stress (σ)
- ^
- | S_ut (Ultimate Tensile Strength)
| * - - .
- | / \
- | S_y (Yield) / \ Fracture (Rupture)
- | *------- *
- | /
- | / <-- Linear Elastic (Slope = E)
- | /
- | /
- | /
- | /
- +----+-----------------------------------------> Strain (ε)
- 0.002 (0.2% Offset)
- Proportional Limit ( σ p l \sigma_{pl} σ pl )
The greatest stress at which stress remains strictly proportional to strain. Below σ p l \sigma_{pl} σ pl , Hooke's law ( σ = E ϵ \sigma = E\epsilon σ = E ϵ ) is valid.
Elastic Limit
The highest stress a material can withstand without undergoing permanent plastic deformation upon complete unloading. In practice, the elastic limit is difficult to measure experimentally and lies just above the proportional limit.
Yield Strength ( S y S_y S y ) & The 0.2% Offset Method
Yield strength defines the stress level at which noticeable plastic deformation begins.
Yield Point Phenomenon: Low-carbon mild steels display distinct upper and lower yield points accompanied by a load drop. This occurs because interstitial carbon and nitrogen solute atoms segregate to dislocations, creating "Cottrell atmospheres" that pin them in place. Once the upper yield point is exceeded, dislocations break free, and Lüders bands propagate across the gage length at the lower yield stress ( S y S_y S y ).
0.2% Offset Yield Strength ( S y S_y S y ): Most structural alloys (including aluminum, copper, titanium, and quenched & tempered alloy steels) exhibit a smooth, continuous transition from elastic to plastic behavior without a distinct yield plateau. For these materials, ASTM E8 specifies the 0.2% offset method :
Locate the strain value ϵ = 0.002 \epsilon = 0.002 ϵ = 0.002 ( 0.2 % 0.2\% 0.2% strain) on the strain axis.
Draw a straight construction line originating at ( 0.002 , 0 ) (0.002, 0) ( 0.002 , 0 ) with a slope equal to Young's Modulus ( E E E ).
The intersection of this offset line with the experimental stress-strain curve defines the 0.2% offset yield strength ( S y S_y S y or R p 0.2 R_{p0.2} R p 0.2 ).
Ultimate Tensile Strength ( S u t S_{ut} S u t )
The maximum engineering stress sustained by the specimen before cross-sectional reduction concentrates into a localized neck:
S u t = P max A 0 S_{ut} = \frac{P_{\max}}{A_0} S u t = A 0 P m a x
Prior to S u t S_{ut} S u t , strain hardening compensates for geometric thinning, allowing the total load P P P to increase uniformly. At S u t S_{ut} S u t , the rate of strain hardening equals the rate of area reduction ( d σ / d ϵ = 0 d\sigma/d\epsilon = 0 d σ / d ϵ = 0 ), initiating plastic instability.
Fracture (Rupture) Strength ( σ f \sigma_f σ f )
The engineering stress at the point of catastrophic separation:
σ f = P f A 0 \sigma_f = \frac{P_f}{A_0} σ f = A 0 P f
Because σ f \sigma_f σ f is calculated using the initial area A 0 A_0 A 0 , it appears significantly lower than S u t S_{ut} S u t on an engineering stress-strain curve. However, the true fracture stress based on the necked area, σ T , f = P f / A f \sigma_{T,f} = P_f / A_f σ T , f = P f / A f , is the highest stress experienced by the material.
4. Energy Absorption Capacities & Ductility Indices
Mechanical energy absorbed during loading is represented by the area under the stress-strain curve, governing spring performance, energy dissipation, and fracture resistance.
Modulus of Resilience ( U r U_r U r )
The modulus of resilience is the elastic strain energy absorbed per unit volume when stressed from zero up to the yield strength without permanent set:
U r = ∫ 0 ϵ y σ d ϵ = 1 2 S y ϵ y = 1 2 S y ( S y E ) = S y 2 2 E U_r = \int_0^{\epsilon_y} \sigma \, d\epsilon = \frac{1}{2} S_y \epsilon_y = \frac{1}{2} S_y \left(\frac{S_y}{E}\right) = \frac{S_y^2}{2E} U r = ∫ 0 ϵ y σ d ϵ = 2 1 S y ϵ y = 2 1 S y ( E S y ) = 2 E S y 2
Units: J/m 3 = N ⋅ m/m 3 = Pa \text{J/m}^3 = \text{N}\cdot\text{m/m}^3 = \text{Pa} J/m 3 = N ⋅ m/m 3 = Pa in SI, or in ⋅ lbf/in 3 = psi \text{in}\cdot\text{lbf/in}^3 = \text{psi} in ⋅ lbf/in 3 = psi in USCS.
Design Significance: U r U_r U r is the primary figure of merit for mechanical springs, flexures, shock-absorbing mounts, and elastic clips. Maximizing elastic energy storage demands materials with high yield strength ( S y S_y S y ) and low modulus of elasticity ( E E E ) , such as heat-treated spring steels, titanium alloys, or beryllium copper.
Modulus of Toughness ( U t U_t U t )
The modulus of toughness is the total mechanical work per unit volume absorbed up to final fracture, represented by the total area under the complete engineering stress-strain curve:
U t = ∫ 0 ϵ f σ d ϵ U_t = \int_0^{\epsilon_f} \sigma \, d\epsilon U t = ∫ 0 ϵ f σ d ϵ
For ductile materials, U t U_t U t is commonly approximated with a trapezoid between yield and ultimate strength; a parabolic stress-strain curve gives the second form:
U t ≈ ( S y + S u t 2 ) ϵ f (ductile metals) , U t ≈ 2 3 S u t ϵ f (parabolic curve) U_t \approx \left(\frac{S_y + S_{ut}}{2}\right) \epsilon_f \quad \text{(ductile metals)}, \qquad U_t \approx \frac{2}{3} S_{ut} \epsilon_f \quad \text{(parabolic curve)} U t ≈ ( 2 S y + S u t ) ϵ f (ductile metals) , U t ≈ 3 2 S u t ϵ f (parabolic curve)
Toughness requires a balance of both strength and ductility . High-strength materials with poor ductility (such as untempered martensitic tool steels) have low toughness, while very soft, weak metals (such as pure lead) also have low toughness despite their ductility.
Ductility Measures: Elongation vs. Reduction of Area
Ductility is the degree of plastic deformation a material sustains before fracture:
Percent Elongation (%EL): % E L = L f − L 0 L 0 × 100 % \%EL = \frac{L_f - L_0}{L_0} \times 100\% % E L = L 0 L f − L 0 × 100% Because %EL includes localized plastic necking, its value depends on the initial gage length. The standard ASTM E8 round specimen ( 0.500 in 0.500\text{ in} 0.500 in diameter) uses a 2.000 in 2.000\text{ in} 2.000 in gage length ( 4 D 4D 4 D ), while ASTM E8M round specimens use 5 D 5D 5 D , so always report elongation together with its gage length.
Percent Reduction of Area (%RA): % R A = A 0 − A f A 0 × 100 % \%RA = \frac{A_0 - A_f}{A_0} \times 100\% % R A = A 0 A 0 − A f × 100% where A f A_f A f is the cross-sectional area at the narrowest section of the fracture neck. Unlike %EL, %RA is independent of specimen gage length and provides a direct measure of the material's true localized plastic strain capability.
Rule of Thumb: Materials exhibiting % E L ≥ 5 % \%EL \ge 5\% % E L ≥ 5% are classified as ductile (governed by shear yielding failure theories like von Mises and Tresca). Materials with % E L < 5 % \%EL < 5\% % E L < 5% are classified as brittle (governed by maximum normal stress and Coulomb-Mohr fracture theories).
5. Comparative Mechanical Properties of Structural Engineering Alloys
The following table summarizes nominal mechanical properties for standard structural alloys at room temperature ( 20 ∘ C / 68 ∘ F 20^\circ\text{C} / 68^\circ\text{F} 2 0 ∘ C /6 8 ∘ F ):
Material Specification Density ρ \rho ρ ( g/cm 3 \text{g/cm}^3 g/cm 3 ) Modulus E E E ( GPa \text{GPa} GPa / Mpsi \text{Mpsi} Mpsi ) Shear Modulus G G G ( GPa \text{GPa} GPa / Mpsi \text{Mpsi} Mpsi ) Poisson's Ratio ν \nu ν Yield Strength S y S_y S y ( MPa \text{MPa} MPa / ksi \text{ksi} ksi ) Tensile Strength S u t S_{ut} S u t ( MPa \text{MPa} MPa / ksi \text{ksi} ksi ) Elongation % E L \%EL % E L ( 2 in 2\text{ in} 2 in , %) Hardness (HBW / HRC)
- ASTM A36 (Structural Carbon Steel) 7.85 200 / 29.0 79.3 / 11.5 0.26 250 / 36.3 400 / 58.0 23 119 HBW
- AISI 1018 (Cold Drawn Mild Steel) 7.85 205 / 29.7 80.0 / 11.6 0.29 370 / 53.7 440 / 63.8 15 126 HBW
- AISI 1045 (Hot Rolled Medium Carbon) 7.85 205 / 29.7 80.0 / 11.6 0.29 310 / 45.0 565 / 81.9 16 163 HBW
- AISI 4140 (Q&T @ 425°C Alloy Steel) 7.85 210 / 30.5 80.0 / 11.6 0.30 1140 / 165 1250 / 181 13 370 HBW / 40 HRC
- AISI 4340 (Q&T @ 315°C Ultra-High) 7.85 210 / 30.5 80.0 / 11.6 0.30 1590 / 231 1720 / 250 10 486 HBW / 50 HRC
AISI 304 (Annealed Austenitic Stainless) 8.00 193 / 28.0 74.0 / 10.7 0.29 205 / 29.7 515 / 74.7 55 140 HBW / 70 HRB
- AISI 410 (Q&T @ 540°C Martensitic SS) 7.75 200 / 29.0 77.0 / 11.2 0.28 700 / 102 900 / 131 16 270 HBW / 28 HRC
- Aluminum 6061-T6 (Structural Al) 2.70 68.9 / 10.0 26.0 / 3.77 0.33 276 / 40.0 310 / 45.0 12 95 HBW / 60 HRB
- Aluminum 7075-T6 (Aerospace Al) 2.81 71.7 / 10.4 26.9 / 3.90 0.33 503 / 73.0 572 / 83.0 11 150 HBW / 87 HRB
- Titanium Ti-6Al-4V (Annealed Grade 5) 4.43 114 / 16.5 44.0 / 6.38 0.31 880 / 128 950 / 138 14 334 HBW / 36 HRC
- Gray Cast Iron Class 30 (Brittle) 7.20 100 / 14.5 40.0 / 5.80 0.25 — (No yield) 214 / 31.0 0.5 210 HBW
Values are representative handbook figures (the quenched-and-tempered 4140 and 4340 rows follow the Shigley Table A-21 tempering data). Design with specification minimums or certified test results, not with typical values.
- 6. Worked Calculation Example: Complete Tensile Test Evaluation
- Problem Statement
A standard cylindrical tensile test specimen machined from an alloy steel bar has an initial diameter d 0 = 0.505 in d_0 = 0.505\text{ in} d 0 = 0.505 in and an initial gage length L 0 = 2.000 in L_0 = 2.000\text{ in} L 0 = 2.000 in . During a tensile test, the following experimental data are recorded:
At an applied tensile load of P 1 = 16 , 000 lbf P_1 = 16,000\text{ lbf} P 1 = 16 , 000 lbf , the elongation is measured as Δ L 1 = 0.0055 in \Delta L_1 = 0.0055\text{ in} Δ L 1 = 0.0055 in (within the linear elastic region).
The 0.2% offset yield load is reached at P y = 21 , 000 lbf P_y = 21,000\text{ lbf} P y = 21 , 000 lbf .
The ultimate tensile load is P max = 28 , 000 lbf P_{\max} = 28,000\text{ lbf} P m a x = 28 , 000 lbf at an elongation of Δ L u = 0.320 in \Delta L_u = 0.320\text{ in} Δ L u = 0.320 in .
The specimen fractures at a rupture load of P f = 22 , 500 lbf P_f = 22,500\text{ lbf} P f = 22 , 500 lbf .
Post-test measurements reveal a final fractured gage length L f = 2.440 in L_f = 2.440\text{ in} L f = 2.440 in and a minimum neck diameter d f = 0.380 in d_f = 0.380\text{ in} d f = 0.380 in .
Poisson's ratio for this alloy is known to be ν = 0.29 \nu = 0.29 ν = 0.29 .
Determine:
The modulus of elasticity ( E E E ) and the modulus of resilience ( U r U_r U r ).
The engineering ultimate tensile strength ( S u t S_{ut} S u t ) and the corresponding true stress ( σ T , u \sigma_{T,u} σ T , u ) and true strain ( ϵ T , u \epsilon_{T,u} ϵ T , u ) at peak load.
The ductility parameters: percent elongation (%EL) and percent reduction of area (%RA).
The shear modulus ( G G G ) of the material.
- Step-by-Step Solution
- Step 1: Initial Cross-Sectional Area
A 0 = π d 0 2 4 = π ( 0.505 in ) 2 4 = 0.2003 in 2 ≈ 0.200 in 2 A_0 = \frac{\pi d_0^2}{4} = \frac{\pi (0.505\text{ in})^2}{4} = 0.2003\text{ in}^2 \approx 0.200\text{ in}^2 A 0 = 4 π d 0 2 = 4 π ( 0.505 in ) 2 = 0.2003 in 2 ≈ 0.200 in 2
Step 2: Modulus of Elasticity ( E E E )
Within the elastic regime at P 1 = 16 , 000 lbf P_1 = 16,000\text{ lbf} P 1 = 16 , 000 lbf : σ 1 = P 1 A 0 = 16 , 000 lbf 0.200 in 2 = 80 , 000 psi = 80.0 ksi \sigma_1 = \frac{P_1}{A_0} = \frac{16,000\text{ lbf}}{0.200\text{ in}^2} = 80,000\text{ psi} = 80.0\text{ ksi} σ 1 = A 0 P 1 = 0.200 in 2 16 , 000 lbf = 80 , 000 psi = 80.0 ksi
ϵ 1 = Δ L 1 L 0 = 0.0055 in 2.000 in = 0.00275 in/in \epsilon_1 = \frac{\Delta L_1}{L_0} = \frac{0.0055\text{ in}}{2.000\text{ in}} = 0.00275\text{ in/in} ϵ 1 = L 0 Δ L 1 = 2.000 in 0.0055 in = 0.00275 in/in
E = σ 1 ϵ 1 = 80 , 000 psi 0.00275 = 29.09 × 10 6 psi ≈ 29.1 Mpsi ( 200.6 GPa ) E = \frac{\sigma_1}{\epsilon_1} = \frac{80,000\text{ psi}}{0.00275} = 29.09 \times 10^6\text{ psi} \approx 29.1\text{ Mpsi} \quad (200.6\text{ GPa}) E = ϵ 1 σ 1 = 0.00275 80 , 000 psi = 29.09 × 1 0 6 psi ≈ 29.1 Mpsi ( 200.6 GPa )
Step 3: Yield Strength ( S y S_y S y ) & Modulus of Resilience ( U r U_r U r )
S y = P y A 0 = 21 , 000 lbf 0.200 in 2 = 105 , 000 psi = 105.0 ksi S_y = \frac{P_y}{A_0} = \frac{21,000\text{ lbf}}{0.200\text{ in}^2} = 105,000\text{ psi} = 105.0\text{ ksi} S y = A 0 P y = 0.200 in 2 21 , 000 lbf = 105 , 000 psi = 105.0 ksi
U r = S y 2 2 E = ( 105 , 000 psi ) 2 2 ( 29.09 × 10 6 psi ) = 1.1025 × 10 10 5.818 × 10 7 ≈ 189.5 in ⋅ lbf/in 3 ( 1.307 MJ/m 3 ) U_r = \frac{S_y^2}{2E} = \frac{(105,000\text{ psi})^2}{2(29.09 \times 10^6\text{ psi})} = \frac{1.1025 \times 10^{10}}{5.818 \times 10^7} \approx 189.5\text{ in}\cdot\text{lbf/in}^3 \quad (1.307\text{ MJ/m}^3) U r = 2 E S y 2 = 2 ( 29.09 × 1 0 6 psi ) ( 105 , 000 psi ) 2 = 5.818 × 1 0 7 1.1025 × 1 0 10 ≈ 189.5 in ⋅ lbf/in 3 ( 1.307 MJ/m 3 )
Step 4: Ultimate Tensile Strength & True State at Peak Load
S u t = P max A 0 = 28 , 000 lbf 0.200 in 2 = 140 , 000 psi = 140.0 ksi S_{ut} = \frac{P_{\max}}{A_0} = \frac{28,000\text{ lbf}}{0.200\text{ in}^2} = 140,000\text{ psi} = 140.0\text{ ksi} S u t = A 0 P m a x = 0.200 in 2 28 , 000 lbf = 140 , 000 psi = 140.0 ksi
The engineering strain at maximum load is: ϵ u = Δ L u L 0 = 0.320 in 2.000 in = 0.160 in/in \epsilon_u = \frac{\Delta L_u}{L_0} = \frac{0.320\text{ in}}{2.000\text{ in}} = 0.160\text{ in/in} ϵ u = L 0 Δ L u = 2.000 in 0.320 in = 0.160 in/in
Assuming constant volume prior to the onset of necking: σ T , u = S u t ( 1 + ϵ u ) = 140.0 ksi × ( 1 + 0.160 ) = 140.0 × 1.160 = 162.4 ksi ( 1120 MPa ) \sigma_{T,u} = S_{ut} (1 + \epsilon_u) = 140.0\text{ ksi} \times (1 + 0.160) = 140.0 \times 1.160 = 162.4\text{ ksi} \quad (1120\text{ MPa}) σ T , u = S u t ( 1 + ϵ u ) = 140.0 ksi × ( 1 + 0.160 ) = 140.0 × 1.160 = 162.4 ksi ( 1120 MPa )
ϵ T , u = ln ( 1 + ϵ u ) = ln ( 1.160 ) ≈ 0.1484 in/in \epsilon_{T,u} = \ln(1 + \epsilon_u) = \ln(1.160) \approx 0.1484\text{ in/in} ϵ T , u = ln ( 1 + ϵ u ) = ln ( 1.160 ) ≈ 0.1484 in/in
Step 5: Ductility Metrics (%EL and %RA)
% E L = L f − L 0 L 0 × 100 % = 2.440 in − 2.000 in 2.000 in × 100 % = 0.440 2.000 × 100 % = 22.0 % \%EL = \frac{L_f - L_0}{L_0} \times 100\% = \frac{2.440\text{ in} - 2.000\text{ in}}{2.000\text{ in}} \times 100\% = \frac{0.440}{2.000} \times 100\% = 22.0\% % E L = L 0 L f − L 0 × 100% = 2.000 in 2.440 in − 2.000 in × 100% = 2.000 0.440 × 100% = 22.0%
The final cross-sectional area at the fracture neck is: A f = π d f 2 4 = π ( 0.380 in ) 2 4 = 0.1134 in 2 A_f = \frac{\pi d_f^2}{4} = \frac{\pi (0.380\text{ in})^2}{4} = 0.1134\text{ in}^2 A f = 4 π d f 2 = 4 π ( 0.380 in ) 2 = 0.1134 in 2
% R A = A 0 − A f A 0 × 100 % = 0.200 in 2 − 0.1134 in 2 0.200 in 2 × 100 % = 0.0866 0.200 × 100 % = 43.3 % \%RA = \frac{A_0 - A_f}{A_0} \times 100\% = \frac{0.200\text{ in}^2 - 0.1134\text{ in}^2}{0.200\text{ in}^2} \times 100\% = \frac{0.0866}{0.200} \times 100\% = 43.3\% % R A = A 0 A 0 − A f × 100% = 0.200 in 2 0.200 in 2 − 0.1134 in 2 × 100% = 0.200 0.0866 × 100% = 43.3%
Because % E L = 22.0 % ≫ 5 % \%EL = 22.0\% \gg 5\% % E L = 22.0% ≫ 5% , the alloy exhibits pronounced ductility.
Step 6: Shear Modulus ( G G G )
G = E 2 ( 1 + ν ) = 29.09 Mpsi 2 ( 1 + 0.29 ) = 29.09 2.58 = 11.28 Mpsi ( 77.8 GPa ) G = \frac{E}{2(1 + \nu)} = \frac{29.09\text{ Mpsi}}{2(1 + 0.29)} = \frac{29.09}{2.58} = 11.28\text{ Mpsi} \quad (77.8\text{ GPa}) G = 2 ( 1 + ν ) E = 2 ( 1 + 0.29 ) 29.09 Mpsi = 2.58 29.09 = 11.28 Mpsi ( 77.8 GPa )