Study guide
2.2 Physical Properties, Temperature Effects, Hardness, Impact Toughness & Creep
PE Mechanical: Machine Design and Materials Exam
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Basic Engineering Practice: Drawings, Economics & Design Methodology
1.1 Engineering Terms, Symbols, Drawing Interpretation & Conventions 1.2 Project Management & Engineering Economics 1.3 Design Methodology, Risk Assessment & Safety
2 Chapter 2: Physical & Mechanical Properties of Engineering Materials
2.1 Stress-Strain Relationships & Fundamental Mechanical Properties 2.2 Physical Properties, Temperature Effects, Hardness, Impact Toughness & Creep
3 Chapter 3: Mechanics of Materials: Fundamental Loadings & Deflections
3.1 Axial Loading, Normal Stress & Statically Indeterminate Members 3.2 Direct Shear, Bearing & Transverse Shear in Beams 3.3 Torsion of Shafts, Power Transmission & Thin-Walled Tubes 3.4 Beam Bending Stresses & Deflection Analysis
4 Chapter 4: Mechanics of Materials: Stability, Multiaxial Stress & Thermal Effects
4.1 Column Buckling & Elastic/Inelastic Instability 4.2 Combined Loading, Principal Stresses & Mohr's Circle 4.3 Thermal Stresses & Interference Stresses
5 Chapter 5: Failure Theories: Static Yielding & Fracture Mechanics
5.1 Static Failure Theories for Ductile Materials: von Mises & Tresca 5.2 Static Failure Theories for Brittle Materials & Fracture Mechanics
6 Chapter 6: Fatigue Analysis & Dynamic Failure
6.1 High-Cycle Fatigue, S-N Curves & Marin Modifying Factors 6.2 Fluctuating Stresses, Failure Criteria & Cumulative Damage
7 Chapter 7: Mechanical Attachments: Fasteners & Bolted Joints
7.1 Threaded Fasteners, Proof Strength & Preload Mechanics 7.2 Bolted Joint Stiffness, External Loading & Separation 7.3 Non-Threaded Fasteners: Keys, Pins, Clevises, Retaining Rings, Rivets, Lugs & Anchors
8 Chapter 8: Mechanical Attachments: Permanent Joints & Bonding
8.1 Welded Joints & Weld Group Stress Analysis 8.2 Brazing, Soldering & Structural Adhesive Bonding
9 Chapter 9: Power Transmission: Shafts & Gearing
9.1 Transmission Shaft Design, Critical Speeds & Deflection 9.2 Spur Gears: Geometry, Kinematics & AGMA Stress Equations 9.3 Helical, Bevel & Worm Gearing
10 Chapter 10: Power Transmission: Bearings, Flexible Drives, Friction Devices & Prime Movers
10.1 Rolling-Element Bearings & L10 Life Calculations 10.2 Hydrodynamic Journal Bearings & Lubrication Regimes 10.3 Belts, Roller Chains & Flexible Drives 10.4 Clutches, Brakes & Power Screws 10.5 Electric Motors, Engines & Flywheels
11 Chapter 11: Mechanical Components: Pressure Vessels & Structural Systems
11.1 Pressure Vessels & Piping: Thin and Thick Walls, ASME VIII and B31 11.2 Mechanical Springs: Helical, Belleville & Leaf Springs 11.3 Structural Trusses, Rigid Frames & Energy Methods
12 Chapter 12: Mechanical Dynamics, Vibrations & Fluid Power
12.1 Single-Degree-of-Freedom Vibrations & Resonance 12.2 Vibration Isolation, Multi-DOF Systems & Transmissibility 12.3 Fluid Power Systems: Hydraulics & Pneumatics
13 Chapter 13: Kinematics, Mechatronics & Control Systems
13.1 Mechanism Kinematics, Linkages, Cams & Simple Machines 13.2 Basic Mechatronics, Sensors & Closed-Loop Controls
14 Chapter 14: Supportive Knowledge: Fits, Tolerances & Manufacturing Methods
14.1 Limits, Fits & Geometric Dimensioning & Tolerancing (GD&T) 14.2 Manufacturing Methods, Machinability, Heat Treatment & Assembly
15 Chapter 15: Supportive Knowledge: Codes, Computation, Testing & Corrosion
15.1 Engineering Codes & Standards 15.2 Computational Methods: FEA & Numerical Analysis 15.3 Instrumentation, Testing, Inspection & Quality 15.4 Chemical Processes: Corrosion, Oxidation & Embrittlement
2.2 Physical Properties, Temperature Effects, Hardness, Impact Toughness & Creep
Key Takeaways Explain This Topic AI
Brinell hardness provides a useful approximate estimate of tensile strength for structural carbon and low-alloy steels: S u t ≈ 500 × HB S_{ut} \approx 500 \times \text{HB} S u t ≈ 500 × HB psi ( 0.50 × HB 0.50 \times \text{HB} 0.50 × HB ksi) or S u t ≈ 3.45 × HB S_{ut} \approx 3.45 \times \text{HB} S u t ≈ 3.45 × HB MPa.
Body-centered cubic (BCC) metals exhibit a pronounced Ductile-to-Brittle Transition Temperature (DBTT), whereas face-centered cubic (FCC) metals (such as austenitic stainless steels and aluminum) retain high impact toughness down to cryogenic temperatures.
Secondary (steady-state) creep ( ϵ ˙ s \dot{\epsilon}_s ϵ ˙ s ) dominates component service life at temperatures above 0.4 T m 0.4 T_m 0.4 T m , representing a dynamic equilibrium between dislocation strain hardening and thermal recovery.
The Larson-Miller parameter ( L M P = T ( C + log 10 t r ) × 10 − 3 LMP = T(C + \log_{10} t_r) \times 10^{-3} L MP = T ( C + lo g 10 t r ) × 1 0 − 3 ) enables short-term elevated-temperature creep rupture data to predict decades-long operating life under identical stress levels.
Physical properties drive many checks: thermal-shock resistance rises with high conductivity and strength and low expansion and modulus, while differential expansion ( α 1 − α 2 ) L Δ T (\alpha_1 - \alpha_2) L \Delta T ( α 1 − α 2 ) L Δ T changes fits with temperature.
Last updated: October 2026
2.2 Temperature Effects, Hardness, Impact Toughness & Creep
Quick Summary: Component performance in operational environments depends on temperature-dependent and time-dependent material degradation mechanisms. This section covers standard hardness testing methodologies (Brinell, Rockwell, Vickers, Knoop) and their empirical correlation to tensile strength in structural steels, analyzes dynamic impact toughness and crystal lattice effects on ductile-to-brittle transitions, and formulates high-temperature creep modeling using the Larson-Miller parameter alongside thermal shock resistance.
1. Hardness Testing Methods & Empirical Correlations
Hardness measures a material's resistance to localized permanent plastic deformation, penetration, abrasion, or scratching. In mechanical engineering, indentation hardness testing provides a rapid, non-destructive means of assessing material strength, quality of heat treatment, and surface wear resistance.
Brinell Hardness Test (ASTM E10)
The Brinell test presses a spherical tungsten carbide ball indenter ( D = 10 mm D = 10\text{ mm} D = 10 mm ) into the specimen surface under a standard static test load P P P :
Standard load: 3000 kgf 3000\text{ kgf} 3000 kgf ( 29.42 kN 29.42\text{ kN} 29.42 kN ) for structural steels and cast irons.
Intermediate load: 1500 kgf 1500\text{ kgf} 1500 kgf for copper alloys and aluminum forgings.
Light load: 500 kgf 500\text{ kgf} 500 kgf for soft aluminum alloys and bearing metals.
The load is sustained for 10 – 15 seconds 10\text{--}15\text{ seconds} 10 – 15 seconds , and the resulting spherical indentation diameter ( d d d ) is measured along two orthogonal axes using an optical microscope:
H B W = 2 P π D ( D − D 2 − d 2 ) HBW = \frac{2P}{\pi D \left(D - \sqrt{D^2 - d^2}\right)} H B W = π D ( D − D 2 − d 2 ) 2 P
where P P P is the applied load in kgf \text{kgf} kgf , D D D is the indenter diameter in mm \text{mm} mm , and d d d is the mean indentation diameter in mm \text{mm} mm .
Engineering Advantage: The large 10 mm 10\text{ mm} 10 mm indenter creates an impression spanning multiple grains, effectively averaging local microstructural variations. This makes Brinell testing the preferred method for cast irons, forgings, hot-rolled structural steel shapes, and coarse-grained weldments.
Designation: E.g., 250 HBW 10/3000 250\text{ HBW 10/3000} 250 HBW 10/3000 denotes a Brinell hardness of 250 250 250 determined with a 10 mm 10\text{ mm} 10 mm tungsten carbide ball under a 3000 kgf 3000\text{ kgf} 3000 kgf load held for 10 – 15 seconds 10\text{--}15\text{ seconds} 10 – 15 seconds .
Rockwell Hardness Test (ASTM E18)
The Rockwell test measures the net permanent increase in indentation depth under a major load relative to an initial minor preload. Unlike the Brinell optical measurement, Rockwell testers provide a direct dial or digital readout:
Preliminary Minor Load ( 10 kgf 10\text{ kgf} 10 kgf ): Applied to seat the indenter through surface scale, oxidation, and surface roughness, establishing a zero-depth datum ( h 0 h_0 h 0 ).
Additional Major Load: Applied and held for the short dwell time specified in ASTM E18, producing plastic penetration.
Major Load Removal: The major load is removed while retaining the minor load. The final permanent indentation depth e e e relative to the datum determines the hardness number: H R = E 0 − e HR = E_0 - e H R = E 0 − e .
Primary Rockwell Scales:
Rockwell C (HRC): 120 ∘ 120^\circ 12 0 ∘ spheroconical diamond Brale indenter, 150 kgf 150\text{ kgf} 150 kgf total load ( 10 kgf 10\text{ kgf} 10 kgf minor + 140 kgf 140\text{ kgf} 140 kgf major). Used for hardened alloy steels, tool steels, quenched and tempered components, and carburized cases exceeding 20 HRC 20\text{ HRC} 20 HRC up to ≈ 70 HRC \approx 70\text{ HRC} ≈ 70 HRC .
Rockwell B (HRB): 1 / 16 in 1/16\text{ in} 1/16 in ( 1.588 mm 1.588\text{ mm} 1.588 mm ) diameter hardened tungsten carbide ball, 100 kgf 100\text{ kgf} 100 kgf total load ( 10 kgf 10\text{ kgf} 10 kgf minor + 90 kgf 90\text{ kgf} 90 kgf major). Used for soft and medium-strength materials: annealed carbon steels, structural aluminum alloys, brass, and bronze ( 0 to 100 HRB 0\text{ to }100\text{ HRB} 0 to 100 HRB ).
Rockwell A (HRA): 120 ∘ 120^\circ 12 0 ∘ diamond Brale indenter, 60 kgf 60\text{ kgf} 60 kgf total load. Used for extremely thin case-hardened surfaces, razor blades, and cemented tungsten carbides to avoid chipping or punching through the thin substrate.
Microhardness: Vickers (HV) & Knoop (HK) (ASTM E384)
When evaluating thin coatings, decarburized surface layers, individual microscopic phases, or heat-affected zones (HAZ) adjacent to welds, microhardness indentations with microscopic depths are required:
Vickers Hardness (HV): Uses a square-based diamond pyramid indenter with an apex face angle of 136 ∘ 136^\circ 13 6 ∘ . Loads range from 1 gf 1\text{ gf} 1 gf to 120 kgf 120\text{ kgf} 120 kgf . The mean diagonal length ( d d d ) of the square impression is measured optically: H V = 2 P sin ( 136 ∘ / 2 ) d 2 ≈ 1.8544 P d 2 HV = \frac{2P \sin(136^\circ/2)}{d^2} \approx 1.8544 \frac{P}{d^2} H V = d 2 2 P s i n ( 13 6 ∘ /2 ) ≈ 1.8544 d 2 P The Vickers scale is continuous from soft pure metals ( 15 HV 15\text{ HV} 15 HV ) to nitrided steels ( 1000 HV 1000\text{ HV} 1000 HV ) and diamond-like coatings ( 2500 HV 2500\text{ HV} 2500 HV ).
Knoop Hardness (HK): Uses an elongated rhombic diamond pyramid indenter with a length-to-width ratio of approximately 7.11 : 1 7.11:1 7.11 : 1 . It produces a shallow, elongated impression that minimizes subsurface cracking in brittle materials (such as glass, ceramics, and intermetallic compounds) and allows precise hardness profiling across narrow case depths.
Empirical Hardness-Strength Correlation for Structural Steels
Because plastic indentation involves localized compressive yielding and shear deformation, hardness correlates directly with ultimate tensile strength for structural steels. Widely used textbook correlations (for example, Shigley gives S u t ≈ 0.5 HB S_{ut} \approx 0.5\,\text{HB} S u t ≈ 0.5 HB kpsi ≈ 3.4 HB \approx 3.4\,\text{HB} ≈ 3.4 HB MPa) are:
- S u t ≈ 500 × HB ( psi ) S_{ut} \approx 500 \times \text{HB} \quad (\text{psi}) S u t ≈ 500 × HB ( psi )
- S u t ≈ 0.50 × HB ( ksi ) S_{ut} \approx 0.50 \times \text{HB} \quad (\text{ksi}) S u t ≈ 0.50 × HB ( ksi )
- S u t ≈ 3.45 × HB ( MPa ) S_{ut} \approx 3.45 \times \text{HB} \quad (\text{MPa}) S u t ≈ 3.45 × HB ( MPa )
Examination Constraints: These linear approximations are estimates for plain carbon and low-alloy steels; they lose accuracy at very low and very high hardness, so treat them as screening values rather than certified strengths. They do not apply to work-hardening austenitic stainless steels, cast irons, or non-ferrous alloys (aluminum, brass, titanium), which have different strain-hardening characteristics.
2. Dynamic Impact Toughness & Fracture Transitions
Under high strain rates, multiaxial constraints, and sub-ambient temperatures, materials that appear ductile in a slow uniaxial tensile test can fail by catastrophic, low-energy brittle fracture without plastic deformation.
Impact Testing: Charpy V-Notch vs. Izod (ASTM E23)
Impact tests measure the mechanical energy absorbed in fracturing a notched specimen struck by a swinging pendulum hammer:
Charpy V-Notch (CVN): The specimen is a 10 mm × 10 mm × 55 mm 10\text{ mm} \times 10\text{ mm} \times 55\text{ mm} 10 mm × 10 mm × 55 mm bar containing a central 45 ∘ 45^\circ 4 5 ∘ , 2 mm 2\text{ mm} 2 mm deep notch with a 0.25 mm 0.25\text{ mm} 0.25 mm root radius. The specimen is supported horizontally at both ends as a simple beam and struck on the face directly opposite the notch.
Izod Test: The specimen is clamped vertically at one end as a cantilever beam and struck above the notch on the same face containing the notch.
The absorbed impact energy ( E abs E_{\text{abs}} E abs ) is computed from the initial release height ( h 0 h_0 h 0 ) and the maximum swing-through height ( h f h_f h f ):
E abs = m g ( h 0 − h f ) E_{\text{abs}} = mg(h_0 - h_f) E abs = m g ( h 0 − h f )
Recorded in Joules ( J \text{J} J ) in SI or foot-pounds ( ft ⋅ lbf \text{ft}\cdot\text{lbf} ft ⋅ lbf ) in USCS ( 1 ft ⋅ lbf = 1.356 J 1\text{ ft}\cdot\text{lbf} = 1.356\text{ J} 1 ft ⋅ lbf = 1.356 J ).
The Ductile-to-Brittle Transition Temperature (DBTT)
When Charpy absorbed energy is plotted as a function of test temperature, ferritic and low-alloy structural steels exhibit a characteristic S-shaped curve: Absorbed Energy
- ^
- | Upper Shelf (Ductile, fibrous microvoid coalescence)
- | -----------------\
- | \
- | \ <-- Transition Region (DBTT)
- | \
- | \-----------------
- | Lower Shelf (Brittle, cleavage fracture)
- +---------------------------------------------------> Temperature (T)
Upper Shelf: At elevated and ambient temperatures, failure occurs by ductile rupture (microvoid nucleation, growth, and coalescence). Fracture surfaces appear dull, fibrous, and display distinct shear lips. Energy absorption is high ( > 50 – 150 J > 50\text{--}150\text{ J} > 50 – 150 J ).
Lower Shelf: At sub-ambient temperatures, failure transitions to rapid transgranular cleavage along crystallographic cleavage planes ( { 100 } \{100\} { 100 } in ferrite). Fracture surfaces appear bright, flat, highly reflective, and crystalline. Energy absorption drops drastically ( < 10 – 15 J < 10\text{--}15\text{ J} < 10 – 15 J ).
Transition Criteria: Design standards (e.g., ASME Boiler and Pressure Vessel Code, ASTM A370) define the DBTT using:
Specific absorbed energy threshold: typically 20 J 20\text{ J} 20 J ( 15 ft ⋅ lbf 15\text{ ft}\cdot\text{lbf} 15 ft ⋅ lbf ) or 27 J 27\text{ J} 27 J ( 20 ft ⋅ lbf 20\text{ ft}\cdot\text{lbf} 20 ft ⋅ lbf ) for structural steels.
Fracture Appearance Transition Temperature (FATT): the temperature at which the fracture surface displays 50% shear (fibrous) and 50% cleavage (crystalline) area.
Lateral expansion threshold: minimum transverse expansion at the specimen's compression face (e.g., ≥ 0.38 mm / 0.015 in \ge 0.38\text{ mm} / 0.015\text{ in} ≥ 0.38 mm /0.015 in ).
Crystal Structure Influence: BCC vs. FCC vs. HCP
The existence of a DBTT is directly dictated by crystal lattice structure and dislocation mobility:
Body-Centered Cubic (BCC) Metals: Carbon steels, low-alloy steels, ferritic/martensitic stainless steels, chromium, molybdenum, and tungsten exhibit a pronounced DBTT . In BCC lattices, dislocation motion (plastic slip) requires overcoming a steep lattice resistance barrier known as the Peierls-Nabarro stress . At lower temperatures, thermal activation energy decreases, the Peierls stress rises exponentially, dislocation motion freezes, and the stress required for slip exceeds the cleavage fracture stress. BCC steels must never be specified for service below their DBTT.
Face-Centered Cubic (FCC) Metals: Austenitic stainless steels (AISI 304, 316), aluminum alloys, copper, nickel, and austenitic nickel-base superalloys do not exhibit a DBTT . FCC crystals possess 12 close-packed slip systems ( { 111 } ⟨ 110 ⟩ \{111\}\langle110\rangle { 111 } ⟨ 110 ⟩ ) with very low Peierls-Nabarro lattice resistance. Dislocation mobility remains active down to cryogenic temperatures ( 4 K / − 269 ∘ C 4\text{ K} / -269^\circ\text{C} 4 K / − 26 9 ∘ C ). FCC alloys maintain exceptional impact toughness, ductility, and resistance to brittle shock at cryogenic temperatures (e.g., liquid nitrogen tanks at − 196 ∘ C -196^\circ\text{C} − 19 6 ∘ C , LNG piping at − 162 ∘ C -162^\circ\text{C} − 16 2 ∘ C , and liquid hydrogen aerospace systems at − 253 ∘ C -253^\circ\text{C} − 25 3 ∘ C ).
Hexagonal Close-Packed (HCP) Metals: Titanium, magnesium, and zinc have limited active slip systems at room temperature, leading to moderate toughness and gradual temperature sensitivity without the steep inflection seen in BCC steels.
3. Elevated Temperature Mechanics: Creep & Stress Rupture
At homologous temperatures exceeding approximately 40 % 40\% 40% of a metal's absolute melting temperature:
T H = T T m > 0.40 ( with T , T m in Kelvin or Rankine ) T_H = \frac{T}{T_m} > 0.40 \quad (\text{with } T, T_m \text{ in Kelvin or Rankine}) T H = T m T > 0.40 ( with T , T m in Kelvin or Rankine )
materials undergo creep —continuous, time-dependent, irreversible plastic deformation under sustained mechanical stress, even when the applied stress is significantly below the static yield strength ( S y S_y S y ).
The Three Stages of Creep
Under constant uniaxial tensile load and constant elevated temperature, a creep curve of strain versus time exhibits three characteristic regimes: Creep Strain (ε)
- ^ Rupture (*)
- | /
- | Stage II / Stage III (Tertiary)
- | (Secondary) /
- | /--------------/
- | Stage I /
- | (Primary) /
- | /-----------/
- | /
- | /
- +----+-----------------------------------------> Time (t)
- Instantaneous
- Elastic Strain (ε_0)
Primary (Transient) Creep (Stage I): Immediately follows elastic deflection. The creep strain rate ( ϵ ˙ = d ϵ / d t \dot{\epsilon} = d\epsilon/dt ϵ ˙ = d ϵ / d t ) decreases continuously over time as dislocation multiplication and forest entanglement produce strain hardening faster than thermal recovery can relieve it.
Secondary (Steady-State) Creep (Stage II): The strain rate reaches a nearly constant minimum value ( ϵ ˙ s \dot{\epsilon}_s ϵ ˙ s ). A dynamic equilibrium is established between strain hardening (dislocation accumulation) and thermal recovery mechanisms (dislocation climb over obstacles, vacancy diffusion, and subgrain boundary migration). Stage II dominates the operational life of engineered components. Steady-state creep rate is modeled by the Norton-Bailey power law : ϵ ˙ s = A σ n exp ( − Q R T ) \dot{\epsilon}_s = A \sigma^n \exp\left(-\frac{Q}{R T}\right) ϵ ˙ s = A σ n exp ( − RT Q ) where A A A is a material constant, σ \sigma σ is the applied stress, n n n is the creep stress exponent (typically 3 ≤ n ≤ 8 3 \le n \le 8 3 ≤ n ≤ 8 for dislocation climb), Q Q Q is the activation energy for creep diffusion ( J/mol \text{J/mol} J/mol ), R R R is the universal gas constant ( 8.314 J/(mol ⋅ K) 8.314\text{ J/(mol}\cdot\text{K)} 8.314 J/(mol ⋅ K) ), and T T T is absolute temperature.
Tertiary Creep (Stage III): The creep rate accelerates rapidly. Grain boundary sliding initiates micro-void cavitation, intergranular cracks propagate, and cross-sectional necking reduces load-bearing area. This instability terminates in catastrophic stress rupture at time t r t_r t r .
The Larson-Miller Parameter (LMP)
Long-term creep rupture testing (e.g., 100 , 000 hours ≈ 11.4 years 100,000\text{ hours} \approx 11.4\text{ years} 100 , 000 hours ≈ 11.4 years ) is impractical during design cycles. The Larson-Miller parameter provides a time-temperature superposition method to extrapolate short-term, accelerated high-temperature test data to predict decades-long operating life at lower service temperatures under identical stress levels:
L M P = T ( C + log 10 t r ) × 10 − 3 LMP = T \left(C + \log_{10} t_r\right) \times 10^{-3} L MP = T ( C + lo g 10 t r ) × 1 0 − 3
Variables & Units:
T T T : Absolute temperature in Rankine ( ∘ R = ∘ F + 459.67 ^\circ\text{R} = ^\circ\text{F} + 459.67 ∘ R = ∘ F + 459.67 ) in USCS practice, or in Kelvin ( K = ∘ C + 273.15 \text{K} = ^\circ\text{C} + 273.15 K = ∘ C + 273.15 ) in SI practice.
t r t_r t r : Time to stress rupture in hours .
C C C : Dimensionless material-specific Larson-Miller constant, typically taken as C = 20 C = 20 C = 20 for structural steels, low-alloy boiler steels, and nickel-base superalloys.
The factor 10 − 3 10^{-3} 1 0 − 3 is conventionally included to scale L M P LMP L MP into a convenient range ( 30 to 60 30\text{ to }60 30 to 60 in ∘ R ⋅ hr ^\circ\text{R}\cdot\text{hr} ∘ R ⋅ hr , or 15 to 35 15\text{ to }35 15 to 35 in K ⋅ hr \text{K}\cdot\text{hr} K ⋅ hr ).
Equivalence Principle: For a given alloy under a specific stress σ \sigma σ , L M P LMP L MP is a constant value. Therefore, a component operating at a lower temperature for a long duration accumulates the same creep damage as an accelerated specimen tested at a higher temperature for a short duration: T 1 ( C + log 10 t r 1 ) = T 2 ( C + log 10 t r 2 ) T_1 \left(C + \log_{10} t_{r1}\right) = T_2 \left(C + \log_{10} t_{r2}\right) T 1 ( C + lo g 10 t r 1 ) = T 2 ( C + lo g 10 t r 2 )
4. Thermal Shock Resistance & Constrained Thermal Stresses
When mechanical equipment undergoes rapid heating or quenching cycles (e.g., steam turbine rotors, brake discs, internal combustion engine cylinder heads), sharp transient temperature gradients induce differential thermal strains.
Constrained Thermal Stresses
For a body subjected to a temperature change Δ T \Delta T Δ T , unconstrained thermal strain is ϵ th = α Δ T \epsilon_{\text{th}} = \alpha \Delta T ϵ th = α Δ T , where α \alpha α is the coefficient of thermal expansion ( m/(m ⋅ ∘ C) \text{m/(m}\cdot^\circ\text{C)} m/(m ⋅ ∘ C) or in/(in ⋅ ∘ F) \text{in/(in}\cdot^\circ\text{F)} in/(in ⋅ ∘ F) ). If the material surface is constrained by colder interior material (or rigid external boundaries), thermal stresses develop:
1D Fully Constrained Bar: σ th = − E α Δ T \sigma_{\text{th}} = -E \alpha \Delta T σ th = − E α Δ T
2D Equibiaxially Constrained Surface (Thermal Shock): σ th = − E α Δ T 1 − ν \sigma_{\text{th}} = -\frac{E \alpha \Delta T}{1 - \nu} σ th = − 1 − ν E α Δ T
During rapid surface cooling (quenching), the surface contracts against the hotter interior, generating severe surface tensile stresses that can initiate surface cracks (thermal crazing or heat checking).
Thermal Shock Resistance Parameters
A material's ability to resist fracture under rapid thermal cycles is characterized by thermal shock parameters:
Severe Thermal Shock (High Biot Number, sudden quench): The surface temperature changes almost instantly, so the allowable temperature jump before surface stress reaches the strength ( σ f \sigma_f σ f for brittle materials, S y S_y S y for ductile metals) is: R = S y ( 1 − ν ) E α R = \frac{S_y (1 - \nu)}{E \alpha} R = E α S y ( 1 − ν )
Mild Thermal Shock (Low Biot Number): Heat conduction inside the part limits the gradient, so thermal conductivity ( k k k ) enters the parameter: R ′ = k S y ( 1 − ν ) E α R' = \frac{k S_y (1 - \nu)}{E \alpha} R ′ = E α k S y ( 1 − ν )
Design Strategy: To maximize thermal shock resistance, engineers select materials with:
High thermal conductivity ( k k k ) to dissipate temperature gradients rapidly.
High tensile/yield strength ( S y S_y S y ) to withstand induced stresses.
Low coefficient of thermal expansion ( α \alpha α ) to minimize thermal strain.
Low modulus of elasticity ( E E E ) to minimize the stress generated per unit thermal strain.
5. Physical Properties Used in Machine Design
Mechanical properties describe how a material resists load. Physical properties describe how heavy it is, how much it expands, and how it stores and conducts heat and electricity. Exam problems combine the two constantly: a shaft-to-housing fit at operating temperature, the inertia of a rotating disk, the temperature rise of a brake rotor, or the resistance of a sensing element.
Material (typical values) Density (g/cm³) Thermal expansion (µm/m per °C) Thermal conductivity (W/m·K) Specific heat (J/kg·K) Melting point or range (°C) Electrical resistivity (µΩ·m)
- 1018 carbon steel 7.87 11.5–12 52 486 about 1,500 0.16
- 304 stainless steel 8.00 17.3 16.2 500 1,400–1,455 0.72
- 6061-T6 aluminum 2.70 23.6 167 896 582–652 0.040
- C11000 copper 8.89 17.0 388 385 1,065–1,083 0.017
- Ti-6Al-4V 4.43 8.6 6.7 526 1,604–1,660 1.78
- Nylon 6/6 (unfilled) 1.14 about 80 0.25 about 1,700 about 265 insulator
How each property enters machine design:
Density ( ρ \rho ρ ) sets mass and rotating inertia ( J = 1 2 m r 2 J = \tfrac{1}{2} m r^2 J = 2 1 m r 2 for a solid disk). Specific stiffness E / ρ E/\rho E / ρ is nearly identical for steel, aluminum and titanium (about 25 GPa per g/cm 3 25\ \text{GPa per g/cm}^3 25 GPa per g/cm 3 ), so switching metals saves weight only when the design is strength-limited, not stiffness-limited.
Coefficient of thermal expansion ( α \alpha α ) gives free growth δ = α L Δ T \delta = \alpha L \Delta T δ = αL Δ T . Mismatched pairs (aluminum housings on steel bearings, polymer bushings on steel shafts) change fits and preloads with temperature.
Thermal conductivity ( k k k ) and thermal diffusivity a = k / ( ρ c p ) a = k/(\rho c_p) a = k / ( ρ c p ) control how fast heat spreads, which matters for brake rotors, welding heat-affected zones and thermal-shock resistance.
Specific heat ( c p c_p c p ) sets the temperature rise when energy is absorbed: Δ T = E / ( m c p ) \Delta T = E/(m c_p) Δ T = E / ( m c p ) .
Melting point or solidus limits brazing and soldering temperatures, and the absolute melting temperature sets the creep threshold ( T > 0.4 T m T > 0.4 T_m T > 0.4 T m ).
Electrical resistivity ( ρ e \rho_e ρ e ) gives conductor resistance R = ρ e L / A R = \rho_e L / A R = ρ e L / A (copper windings, heater elements, strain-gage alloys). Ferritic and martensitic steels are ferromagnetic , while austenitic stainless steels, aluminum and copper are not, which decides whether magnetic particle inspection or magnetic sensors can be used.
Tip
Worked mini-example (thermal fit change): A steel bearing outer ring ( α = 11.5 × 10 − 6 / ∘ C \alpha = 11.5 \times 10^{-6}/^\circ\text{C} α = 11.5 × 1 0 − 6 / ∘ C ) sits in a 6061 aluminum housing bore ( α = 23.6 × 10 − 6 / ∘ C \alpha = 23.6 \times 10^{-6}/^\circ\text{C} α = 23.6 × 1 0 − 6 / ∘ C ) with 0.020 mm 0.020\,\text{mm} 0.020 mm interference at 20 ∘ C 20^\circ\text{C} 2 0 ∘ C . Both parts have a 72.000 mm 72.000\,\text{mm} 72.000 mm nominal diameter. At 90 ∘ C 90^\circ\text{C} 9 0 ∘ C ( Δ T = 70 ∘ C \Delta T = 70^\circ\text{C} Δ T = 7 0 ∘ C ) the bore grows 0.061 mm 0.061\,\text{mm} 0.061 mm more than the ring: ( 23.6 − 11.5 ) × 10 − 6 × 72 × 70 = 0.061 mm (23.6 - 11.5) \times 10^{-6} \times 72 \times 70 = 0.061\,\text{mm} ( 23.6 − 11.5 ) × 1 0 − 6 × 72 × 70 = 0.061 mm . The fit becomes about 0.041 mm 0.041\,\text{mm} 0.041 mm clearance , so the outer ring can creep and fret. Designers respond with tighter room-temperature fits, steel liners or anti-rotation features.
- 6. Worked Numerical Examples
- Example 1: Brinell Hardness & Shaft Strength Estimation
Problem: A transmission intermediate shaft machined from AISI 4140 alloy steel undergoes Brinell quality verification. A 10 mm 10\text{ mm} 10 mm tungsten carbide ball under a 3000 kgf 3000\text{ kgf} 3000 kgf load produces a spherical indentation with an average diameter d = 3.80 mm d = 3.80\text{ mm} d = 3.80 mm .
Calculate the Brinell Hardness Number ( H B W HBW H B W ).
Estimate the ultimate tensile strength ( S u t S_{ut} S u t ) in both ksi \text{ksi} ksi and MPa \text{MPa} MPa .
Solution:
Brinell hardness calculation: H B W = 2 P π D ( D − D 2 − d 2 ) HBW = \frac{2P}{\pi D \left(D - \sqrt{D^2 - d^2}\right)} H B W = π D ( D − D 2 − d 2 ) 2 P Substitute P = 3000 kgf P = 3000\text{ kgf} P = 3000 kgf , D = 10 mm D = 10\text{ mm} D = 10 mm , and d = 3.80 mm d = 3.80\text{ mm} d = 3.80 mm : D 2 − d 2 = 10 2 − 3.80 2 = 100 − 14.44 = 85.56 = 9.2499 mm \sqrt{D^2 - d^2} = \sqrt{10^2 - 3.80^2} = \sqrt{100 - 14.44} = \sqrt{85.56} = 9.2499\text{ mm} D 2 − d 2 = 1 0 2 − 3.8 0 2 = 100 − 14.44 = 85.56 = 9.2499 mm D − D 2 − d 2 = 10 − 9.2499 = 0.7501 mm D - \sqrt{D^2 - d^2} = 10 - 9.2499 = 0.7501\text{ mm} D − D 2 − d 2 = 10 − 9.2499 = 0.7501 mm H B W = 2 ( 3000 ) π ( 10 ) ( 0.7501 ) = 6000 23.565 ≈ 254.6 ≈ 255 HBW HBW = \frac{2(3000)}{\pi (10)(0.7501)} = \frac{6000}{23.565} \approx 254.6 \approx 255\text{ HBW} H B W = π ( 10 ) ( 0.7501 ) 2 ( 3000 ) = 23.565 6000 ≈ 254.6 ≈ 255 HBW
Tensile strength estimation:
Using the empirical correlation for low-alloy structural steels: S u t ≈ 500 × HB psi = 0.50 × 255 = 127.5 ksi S_{ut} \approx 500 \times \text{HB} \text{ psi} = 0.50 \times 255 = 127.5\text{ ksi} S u t ≈ 500 × HB psi = 0.50 × 255 = 127.5 ksi In SI units: S u t ≈ 3.45 × HB MPa = 3.45 × 255 = 879.8 MPa ≈ 880 MPa S_{ut} \approx 3.45 \times \text{HB} \text{ MPa} = 3.45 \times 255 = 879.8\text{ MPa} \approx 880\text{ MPa} S u t ≈ 3.45 × HB MPa = 3.45 × 255 = 879.8 MPa ≈ 880 MPa
Example 2: Boiler Superheater Tube Creep Rupture Life Evaluation
Problem: An alloy steel superheater tube in an industrial boiler operates at a sustained internal pressure generating a hoop stress of σ = 120 MPa \sigma = 120\text{ MPa} σ = 120 MPa .
In an accelerated laboratory creep rupture test conducted at T 1 = 650 ∘ C T_1 = 650^\circ\text{C} T 1 = 65 0 ∘ C under the same stress of 120 MPa 120\text{ MPa} 120 MPa , the specimen ruptured after t r 1 = 250 hours t_{r1} = 250\text{ hours} t r 1 = 250 hours .
The material follows the Larson-Miller parameter with C = 20 C = 20 C = 20 , where T T T is in Kelvin: L M P = T ( 20 + log 10 t r ) × 10 − 3 LMP = T \left(20 + \log_{10} t_r\right) \times 10^{-3} L MP = T ( 20 + lo g 10 t r ) × 1 0 − 3
Determine:
The Larson-Miller parameter ( L M P LMP L MP ) for this stress level.
The expected operational service life ( t r 2 t_{r2} t r 2 ) in hours and years if the tube operates at T 2 = 550 ∘ C T_2 = 550^\circ\text{C} T 2 = 55 0 ∘ C .
Solution:
Convert test temperature to Kelvin: T 1 = 650 ∘ C + 273.15 = 923.15 K T_1 = 650^\circ\text{C} + 273.15 = 923.15\text{ K} T 1 = 65 0 ∘ C + 273.15 = 923.15 K Calculate log 10 t r 1 \log_{10} t_{r1} lo g 10 t r 1 : log 10 ( 250 ) ≈ 2.3979 \log_{10}(250) \approx 2.3979 lo g 10 ( 250 ) ≈ 2.3979 Calculate L M P LMP L MP : L M P = 923.15 × ( 20 + 2.3979 ) × 10 − 3 = 923.15 × 22.3979 × 10 − 3 = 20.6767 LMP = 923.15 \times (20 + 2.3979) \times 10^{-3} = 923.15 \times 22.3979 \times 10^{-3} = 20.6767 L MP = 923.15 × ( 20 + 2.3979 ) × 1 0 − 3 = 923.15 × 22.3979 × 1 0 − 3 = 20.6767
Calculate service life at T 2 = 550 ∘ C T_2 = 550^\circ\text{C} T 2 = 55 0 ∘ C : T 2 = 550 ∘ C + 273.15 = 823.15 K T_2 = 550^\circ\text{C} + 273.15 = 823.15\text{ K} T 2 = 55 0 ∘ C + 273.15 = 823.15 K Because the stress level is unchanged ( σ = 120 MPa \sigma = 120\text{ MPa} σ = 120 MPa ), L M P LMP L MP remains invariant ( L M P = 20.6767 LMP = 20.6767 L MP = 20.6767 ): 823.15 × ( 20 + log 10 t r 2 ) × 10 − 3 = 20.6767 823.15 \times \left(20 + \log_{10} t_{r2}\right) \times 10^{-3} = 20.6767 823.15 × ( 20 + lo g 10 t r 2 ) × 1 0 − 3 = 20.6767 20 + log 10 t r 2 = 20.6767 × 10 3 823.15 = 20676.7 823.15 ≈ 25.1190 20 + \log_{10} t_{r2} = \frac{20.6767 \times 10^3}{823.15} = \frac{20676.7}{823.15} \approx 25.1190 20 + lo g 10 t r 2 = 823.15 20.6767 × 1 0 3 = 823.15 20676.7 ≈ 25.1190 log 10 t r 2 = 25.1190 − 20 = 5.1190 \log_{10} t_{r2} = 25.1190 - 20 = 5.1190 lo g 10 t r 2 = 25.1190 − 20 = 5.1190 t r 2 = 10 5.1190 ≈ 131 , 520 hours t_{r2} = 10^{5.1190} \approx 131,520\text{ hours} t r 2 = 1 0 5.1190 ≈ 131 , 520 hours
Converting operating hours to years (assuming continuous operation at 8 , 760 hours/year 8,760\text{ hours/year} 8 , 760 hours/year ): Life = 131 , 520 hours 8 , 760 hours/year ≈ 15.0 years \text{Life} = \frac{131,520\text{ hours}}{8,760\text{ hours/year}} \approx 15.0\text{ years} Life = 8 , 760 hours/year 131 , 520 hours ≈ 15.0 years
Engineering Takeaway: Reducing the operating temperature by 100 ∘ C 100^\circ\text{C} 10 0 ∘ C (from 650 ∘ C 650^\circ\text{C} 65 0 ∘ C to 550 ∘ C 550^\circ\text{C} 55 0 ∘ C ) increases component rupture life from approximately 10 days 10\text{ days} 10 days ( 250 hours 250\text{ hours} 250 hours ) to 15 years 15\text{ years} 15 years ( 131 , 520 hours 131,520\text{ hours} 131 , 520 hours ). This highlights the exponential sensitivity of creep rupture life to operating temperature.