8.2 Phase Diagrams, Iron-Carbon System & Heat Treatment
PRC Mechanical Engineer Licensure Examination MELE
Track your progress as you read
Finished sections get a check mark.
1 Chapter 1: Licensing Overview, Law & Professional Ethics
1.1 MELE Facts, RA 8495 & Board Organization 1.2 Code of Ethics for Mechanical Engineers & Professional Practice 1.3 Philippine Mechanical Engineering Code (PME Code) Governance & Legal Mandates
2 Chapter 2: Advanced Mathematics & Engineering Statistics
2.1 Differential & Integral Calculus in Engineering Applications 2.2 Differential Equations & Mathematical Modeling 2.3 Applied Engineering Statistics & Quality Control Probability
3 Chapter 3: Engineering Thermodynamics
3.1 Thermodynamic State Postulate, Properties & P-V-T Equations of State 3.2 First Law Analysis for Open & Closed Thermal Systems 3.3 Second Law, Entropy, Exergy & Reversibility Analysis
4 Chapter 4: Fluid Mechanics & Hydraulic Engineering
4.1 Fluid Statics, Manometry, Hydrostatic Force & Buoyancy 4.2 Fluid Kinematics, Dynamics & Bernoulli Equation 4.3 Pipe Flow, Friction Losses & Piping Network Analysis
5 Chapter 5: Heat Transfer & Thermal Systems
5.1 Conduction Heat Transfer & Thermal Insulation Design 5.2 Natural & Forced Convection Heat Transfer Correlations 5.3 Thermal Radiation & Industrial Heat Exchanger Design
6 Chapter 6: Mechanics & Strength of Materials
6.1 Statics & Dynamics of Rigid Bodies & Engineering Linkages 6.2 Normal, Shear & Triaxial Stress-Strain Relationships 6.3 Bending Stresses, Torsion & Column Buckling Analysis
7 Chapter 7: Engineering Economics & Financial Analysis
7.1 Time Value of Money & Cash Flow Equivalence Formulas 7.2 Asset Depreciation, Taxation & Economic Evaluation Methods 7.3 Break-Even Analysis, Payback Period & EOQ Inventory Models
8 Chapter 8: Engineering Materials & Metallurgy
8.1 Ferrous & Non-Ferrous Metals, Alloys & Polymers 8.2 Phase Diagrams, Iron-Carbon System & Heat Treatment 8.3 Mechanical Testing, Fatigue Failure & Fracture Mechanics
9 Chapter 9: Machine Elements & Stress Analysis
9.1 Failure Theories, Static & Fluctuating Stress Design 9.2 Power Transmission Shafts, Keys & Rigid/Flexible Couplings 9.3 Spur, Helical, Bevel & Worm Gear Design Calculations
10 Chapter 10: Power Transmission Components
10.1 Belts, V-Belts, Chains, Wire Ropes & Flywheels 10.2 Rolling Element & Hydrodynamic Journal Bearings 10.3 Mechanical Springs, Clutches & Industrial Brakes
11 Chapter 11: Manufacturing, Fasteners & GD&T
11.1 Threaded Fasteners, Rivets & Welded Joint Analysis 11.2 Manufacturing Processes, Machine Tools & Machining Calculations 11.3 Engineering Drawing, Limits, Fits, Tolerances & GD&T
12 Chapter 12: Power Plants, Boilers & Thermal Power Cycles
12.1 Steam Power Plants & Rankine Cycles 12.2 Steam Generators, Boilers & Combustion Engineering 12.3 Internal Combustion Engines: SI & CI Cycles 12.4 Gas Turbine Power Plants & Combined Cycles
13 Chapter 13: Renewable Energy, Fluid Machinery & Plant Systems
13.1 Hydroelectric, Geothermal & Renewable Energy Power Plants 13.2 Pumps & Hydraulic Machinery 13.3 Air Compressors, Fans & Blowers
14 Chapter 14: Refrigeration, HVAC & Building Mechanical Systems
14.1 Refrigeration Systems, Cycles & Refrigerants 14.2 Psychrometrics & Air Conditioning Systems 14.3 Piping/Ductwork Design, PME Code & Industrial Safety Management
8.2 Phase Diagrams, Iron-Carbon System & Heat Treatment
Key Takeaways Explain This Topic AI
Gibbs Phase Rule ( F = C − P + 2 F = C - P + 2 F = C − P + 2 , or F = C − P + 1 F = C - P + 1 F = C − P + 1 at constant pressure) defines the degrees of freedom in alloy equilibrium systems.
The Iron-Iron Carbide phase diagram features key invariant points: the eutectic point at 4.3% C ( 1148 ∘ C 1148^\circ\text{C} 114 8 ∘ C forming Ledeburite) and the eutectoid point at 0.77% C ( 727 ∘ C 727^\circ\text{C} 72 7 ∘ C forming Pearlite).
The Lever Rule determines the weight fractions of phases in a two-phase field: W α = C β − C 0 C β − C α W_\alpha = \frac{C_\beta - C_0}{C_\beta - C_\alpha} W α = C β − C α C β − C 0 .
Full annealing involves slow furnace cooling to produce coarse pearlite, while normalizing relies on air cooling to produce fine pearlite with higher yield strength.
Quenching traps carbon in a body-centered tetragonal (BCT) lattice forming hard, brittle martensite; subsequent tempering restores toughness by precipitating fine carbides.
Last updated: July 2026
8.2 Phase Diagrams, Iron-Carbon System & Heat Treatment
PRC MELE Core Focus: Phase diagrams and thermal processing are heavily tested in the MELE board exam. Mechanical engineers must be able to read equilibrium phase diagrams, perform lever rule calculations, identify invariant phase reactions, explain microstructural constituents ( F e 3 C Fe_3C F e 3 C , α \alpha α , γ \gamma γ , pearlite, martensite), and select appropriate heat treatment parameters (annealing, normalizing, hardening, tempering, surface hardening).
1. Phase Diagram Fundamentals & Gibbs Phase Rule
A phase diagram is a graphical representation of the phases present in an alloy system at equilibrium as a function of temperature, pressure, and chemical composition.
Gibbs Phase Rule
The number of operational degrees of freedom ( F F F ) for a system at equilibrium is given by Gibbs Phase Rule: F = C − P + 2 F = C - P + 2 F = C − P + 2
where:
F F F = Degrees of freedom (number of internally controllable variables: temperature, pressure, composition).
C C C = Number of components (elements or chemically independent species, e.g., F e Fe F e and C C C , so C = 2 C = 2 C = 2 for binary systems).
P P P = Number of phases coexisting at equilibrium.
For condensed-phase metallurgical systems operating at constant atmospheric pressure ( 1 atm 1\text{ atm} 1 atm ), the pressure degree of freedom is fixed, yielding the Condensed Gibbs Phase Rule : F = C − P + 1 F = C - P + 1 F = C − P + 1
In a binary system ( C = 2 C = 2 C = 2 ):
In a single-phase field ( P = 1 P = 1 P = 1 ): F = 2 − 1 + 1 = 2 F = 2 - 1 + 1 = 2 F = 2 − 1 + 1 = 2 (both temperature and composition can vary independently).
In a two-phase field ( P = 2 P = 2 P = 2 ): F = 2 − 2 + 1 = 1 F = 2 - 2 + 1 = 1 F = 2 − 2 + 1 = 1 (univariant: specifying temperature fixes phase compositions).
At an invariant point ( P = 3 P = 3 P = 3 ): F = 2 − 3 + 1 = 0 F = 2 - 3 + 1 = 0 F = 2 − 3 + 1 = 0 (invariant: zero degrees of freedom; reaction occurs at a unique temperature and composition).
Lever Rule
In a two-phase field containing phases α \alpha α and β \beta β , the tie-line construction and lever rule determine the weight fraction ( W W W ) of each phase for an alloy of overall composition C 0 C_0 C 0 : W α = C β − C 0 C β − C α W\alpha = \frac{C_\beta - C_0}{C_\beta - C\alpha} W α = C β − C α C β − C 0 W β = C 0 − C α C β − C α = 1 − W α W_\beta = \frac{C_0 - C\alpha}{C_\beta - C\alpha} = 1 - W\alpha W β = C β − C α C 0 − C α = 1 − W α
where C α C_\alpha C α and C β C_\beta C β are the phase boundary compositions at the tie-line temperature.
2. The Iron-Iron Carbide ( F e − F e 3 C Fe-Fe_3C F e − F e 3 C ) Equilibrium Diagram
The F e − F e 3 C Fe-Fe_3C F e − F e 3 C system extends from pure iron ( 0 % C 0\% \text{ C} 0% C ) to the intermetallic compound Cementite ( F e 3 C Fe_3C F e 3 C , 6.70 wt % C 6.70\text{ wt}\% \text{ C} 6.70 wt % C ) .
Key Phases
α \alpha α -Ferrite (Ferrite): Solid solution of carbon in Body-Centered Cubic (BCC) iron. Stable up to 912 ∘ C 912^\circ\text{C} 91 2 ∘ C . Maximum carbon solubility is extremely low: 0.022 wt % C 0.022\text{ wt}\% \text{ C} 0.022 wt % C at 727 ∘ C 727^\circ\text{C} 72 7 ∘ C (drops to 0.008 % 0.008\% 0.008% at room temperature). Soft, ductile, magnetic.
γ \gamma γ -Austenite (Austenite): Solid solution of carbon in Face-Centered Cubic (FCC) iron. Stable between 727 ∘ C 727^\circ\text{C} 72 7 ∘ C and 1394 ∘ C 1394^\circ\text{C} 139 4 ∘ C . Maximum carbon solubility is 2.14 wt % C 2.14\text{ wt}\% \text{ C} 2.14 wt % C at 1148 ∘ C 1148^\circ\text{C} 114 8 ∘ C . Non-magnetic, highly formable.
Cementite ( F e 3 C Fe_3C F e 3 C ): Hard, brittle intermetallic compound containing 6.70 wt % C 6.70\text{ wt}\% \text{ C} 6.70 wt % C . Crystal structure is complex orthorhombic. Hardness ≈ 68 − 70 HRC \approx 68-70\text{ HRC} ≈ 68 − 70 HRC .
δ \delta δ -Ferrite: High-temperature BCC solid solution stable between 1394 ∘ C 1394^\circ\text{C} 139 4 ∘ C and 1538 ∘ C 1538^\circ\text{C} 153 8 ∘ C (melting point of pure iron). Max carbon solubility 0.09 % 0.09\% 0.09% at 1495 ∘ C 1495^\circ\text{C} 149 5 ∘ C .
3. Invariant Reactions in the F e − F e 3 C Fe-Fe_3C F e − F e 3 C System
Three distinct invariant reactions occur on the F e − F e 3 C Fe-Fe_3C F e − F e 3 C phase diagram:
Invariant Reaction Type Temperature Carbon Content Reaction Equation Resulting Microstructure
Eutectic Reaction Liquid → \rightarrow → 2 Solids 1148 ∘ C 1148^\circ\text{C} 114 8 ∘ C 4.30 wt % C 4.30\text{ wt}\% \text{ C} 4.30 wt % C L 4.3 % ⇌ γ 2.14 % + F e 3 C 6.7 % L_{4.3\%} \rightleftharpoons \gamma_{2.14\%} + Fe_3C_{6.7\%} L 4.3% ⇌ γ 2.14% + F e 3 C 6.7% Ledeburite (Eutectic mixture of austenite and cementite)
Eutectoid Reaction Solid → \rightarrow → 2 Solids 727 ∘ C 727^\circ\text{C} 72 7 ∘ C ( A 1 A_1 A 1 ) 0.77 wt % C 0.77\text{ wt}\% \text{ C} 0.77 wt % C γ 0.77 % ⇌ α 0.022 % + F e 3 C 6.7 % \gamma_{0.77\%} \rightleftharpoons \alpha_{0.022\%} + Fe_3C_{6.7\%} γ 0.77% ⇌ α 0.022% + F e 3 C 6.7% Pearlite (Alternating lamellae of ferrite and cementite)
Peritectic Reaction Liquid + Solid → \rightarrow → Solid 1495 ∘ C 1495^\circ\text{C} 149 5 ∘ C 0.16 wt % C 0.16\text{ wt}\% \text{ C} 0.16 wt % C δ 0.09 % + L 0.53 % ⇌ γ 0.17 % \delta_{0.09\%} + L_{0.53\%} \rightleftharpoons \gamma_{0.17\%} δ 0.09% + L 0.53% ⇌ γ 0.17% Austenite ( γ \gamma γ )
Classification of Steels and Cast Irons
Hypoeutectoid Steels: < 0.77 wt % C < 0.77\text{ wt}\% \text{ C} < 0.77 wt % C (microstructure consists of proeutectoid ferrite + pearlite).
Eutectoid Steel: Exactly 0.77 wt % C 0.77\text{ wt}\% \text{ C} 0.77 wt % C (microstructure is 100 % 100\% 100% pearlite).
Hypereutectoid Steels: 0.77 % to 2.14 wt % C 0.77\% \text{ to } 2.14\text{ wt}\% \text{ C} 0.77% to 2.14 wt % C (microstructure consists of proeutectoid cementite + pearlite).
Cast Irons: > 2.14 wt % C > 2.14\text{ wt}\% \text{ C} > 2.14 wt % C up to 6.70 wt % C 6.70\text{ wt}\% \text{ C} 6.70 wt % C (typically 2.5 − 4.0 wt % C 2.5 - 4.0\text{ wt}\% \text{ C} 2.5 − 4.0 wt % C ).
4. Heat Treatment Processes
Heat treatment is the controlled heating and cooling of metals in the solid state to alter mechanical properties, refine microstructures, or relieve internal stresses.
Bulk Heat Treatments
Full Annealing:
Procedure: Heating hypoeutectoid steel 30 − 50 ∘ C 30-50^\circ\text{C} 30 − 5 0 ∘ C above A 3 A_3 A 3 line (or hypereutectoid steel above A 1 A_1 A 1 ), holding, followed by very slow furnace cooling ( 10 − 30 ∘ C/hr 10-30^\circ\text{C/hr} 10 − 3 0 ∘ C/hr ).
Microstructure: Coarse pearlite + proeutectoid ferrite/cementite.
Purpose: Minimum hardness, maximum ductility, stress relief, optimum machinability.
Normalizing:
Procedure: Heating 30 − 50 ∘ C 30-50^\circ\text{C} 30 − 5 0 ∘ C above A 3 A_3 A 3 (hypoeutectoid) or A c m A_{cm} A c m (hypereutectoid), holding, followed by cooling in still air .
Microstructure: Fine pearlite with refined grain size.
Purpose: Higher yield strength, UTS, and hardness than full annealing; eliminates columnar grains and forging segregation.
Process Annealing & Stress-Relief Annealing:
Process Annealing: Subcritical heating ( 550 − 650 ∘ C 550-650^\circ\text{C} 550 − 65 0 ∘ C , below A 1 A_1 A 1 ) to soften cold-worked low-carbon steel sheet/wire via recrystallization.
Stress-Relief Annealing: Subcritical heating ( 500 − 650 ∘ C 500-650^\circ\text{C} 500 − 65 0 ∘ C ) to relieve residual stresses from machining, welding, or casting without phase transformation.
Quenching (Hardening):
Procedure: Austenitizing above A 3 A_3 A 3 , followed by rapid cooling in water, brine, or oil faster than the critical cooling rate.
Mechanism: Suppresses carbon diffusion; FCC austenite transforms via diffusionless shear reaction into Martensite (Body-Centered Tetragonal, BCT, supersaturated solid solution of carbon in iron).
Properties: Extremely high hardness ( 60 − 65 HRC 60-65\text{ HRC} 60 − 65 HRC ), low toughness, high internal stress, extreme brittleness.
Tempering:
Procedure: Reheating quenched martensitic steel to subcritical temperatures ( 150 − 650 ∘ C 150-650^\circ\text{C} 150 − 65 0 ∘ C ) for 1 − 2 hours 1-2\text{ hours} 1 − 2 hours , followed by air cooling.
Microstructure: Tempered Martensite (extremely fine dispersion of F e 3 C Fe_3C F e 3 C particles in a ferrite matrix).
Effect: Reduces brittleness, relieves internal stresses, and restores toughness and impact strength while slightly reducing hardness.
Low Tempering ( 150 − 250 ∘ C 150-250^\circ\text{C} 150 − 25 0 ∘ C ): Relieves stress ( 58 − 62 HRC 58-62\text{ HRC} 58 − 62 HRC , cutting tools).
Medium Tempering ( 350 − 500 ∘ C 350-500^\circ\text{C} 350 − 50 0 ∘ C ): High elastic limit, spring steel ( 40 − 50 HRC 40-50\text{ HRC} 40 − 50 HRC ).
High Tempering ( 500 − 650 ∘ C 500-650^\circ\text{C} 500 − 65 0 ∘ C ): High toughness and fatigue strength ( 25 − 35 HRC 25-35\text{ HRC} 25 − 35 HRC , shafts, gears).
5. Surface & Case Hardening Methods
When components require a hard, wear-resistant outer surface (case) backed by a ductile, tough interior (core) to absorb impact loads (e.g., gears, shafts, camshafts):
Carburizing (Pack, Gas, Liquid): Carbon diffusion into low-carbon steel ( 0.15 − 0.25 % C 0.15-0.25\% \text{ C} 0.15 − 0.25% C ) surface at 900 − 950 ∘ C 900-950^\circ\text{C} 900 − 95 0 ∘ C in a carbonaceous environment (CO gas or liquid cyanide bath). Case depth up to 1.5 − 2.0 mm 1.5-2.0\text{ mm} 1.5 − 2.0 mm , followed by quenching and tempering.
Nitriding: Nitrogen diffusion into special alloy steel containing Al , Cr , Mo \text{Al}, \text{Cr}, \text{Mo} Al , Cr , Mo at subcritical temperatures ( 500 − 550 ∘ C 500-550^\circ\text{C} 500 − 55 0 ∘ C ) using ammonia gas ( NH 3 \text{NH}_3 NH 3 ). Forms extremely hard alloy nitrides ( ≈ 68 − 72 HRC \approx 68-72\text{ HRC} ≈ 68 − 72 HRC ). No quenching required , producing minimal distortion.
Cyaniding & Carbonitriding: Simultaneous diffusion of carbon and nitrogen at 800 − 870 ∘ C 800-870^\circ\text{C} 800 − 87 0 ∘ C in a molten cyanide salt bath or gas atmosphere.
Induction Hardening & Flame Hardening: Localized surface heating of medium-carbon steels ( 0.40 − 0.50 % C 0.40-0.50\% \text{ C} 0.40 − 0.50% C ) via high-frequency electromagnetic induction coils or oxy-acetylene flames above A 3 A_3 A 3 , immediately followed by direct water spray quenching. Chemical composition of core and surface remains unchanged.
- 6. TTT Diagrams & Hardenability
- Time-Temperature-Transformation (TTT / Isothermal) Diagrams
TTT curves plot temperature vs. logarithmic time for isothermal phase transformations of austenite. Key features:
Nose of the TTT Curve: Minimum time required for Pearlite transformation to begin (around 550 ∘ C 550^\circ\text{C} 55 0 ∘ C ).
Pearlite Region ( 727 − 550 ∘ C 727 - 550^\circ\text{C} 727 − 55 0 ∘ C ): High temperatures yield coarse pearlite; lower temperatures near the nose yield fine pearlite.
Bainite Region ( 550 − 250 ∘ C 550 - 250^\circ\text{C} 550 − 25 0 ∘ C ): Formed by isothermal transformation between the nose and M s M_s M s temperature. Microstructure consists of non-lamellar needle-like ferrite and fine F e 3 C Fe_3C F e 3 C precipitates ( Upper Bainite at 400 − 550 ∘ C 400-550^\circ\text{C} 400 − 55 0 ∘ C , Lower Bainite at 250 − 400 ∘ C 250-400^\circ\text{C} 250 − 40 0 ∘ C ).
Martensite Start ( M s M_s M s ) & Finish ( M f M_f M f ) Lines: Athermal transformation lines. M s ≈ 220 ∘ C M_s \approx 220^\circ\text{C} M s ≈ 22 0 ∘ C for 0.80 % C 0.80\% \text{ C} 0.80% C steel.
Hardenability & The Jominy End-Quench Test
Hardenability: The depth to which a steel alloy can be hardened by martensitic transformation upon quenching (distinct from maximum hardness, which depends purely on carbon content).
Jominy End-Quench Test (ASTM A255): A standard 25.4 mm 25.4\text{ mm} 25.4 mm diameter × 101.6 mm \times 101.6\text{ mm} × 101.6 mm long specimen is austenitized, placed in a fixture, and quenched at one end by a controlled water jet. Hardness is measured along the length at 1 / 16 inch 1/16\text{ inch} 1/16 inch intervals. Alloy steels (e.g., 4340) maintain high hardness deep along the bar due to high hardenability, whereas plain carbon steels (1045) show a rapid drop in hardness away from the quenched end.
7. Worked Engineering Calculation
Problem: A 0.45 wt % C 0.45\text{ wt}\% \text{ C} 0.45 wt % C plain carbon steel is slowly cooled from 900 ∘ C 900^\circ\text{C} 90 0 ∘ C to just below the eutectoid temperature ( 727 ∘ C − Δ T 727^\circ\text{C} - \Delta T 72 7 ∘ C − Δ T ).
Calculate:
The weight fraction of proeutectoid ferrite ( W α ′ W_{\alpha'} W α ′ ) formed prior to the eutectoid transformation.
The weight fraction of total ferrite ( W α , total W_{\alpha, \text{total}} W α , total ) at room temperature.
The weight fraction of pearlite ( W P W_P W P ) present at room temperature.
Given data: Carbon solubility in ferrite C α = 0.022 wt % C C_\alpha = 0.022\text{ wt}\% \text{ C} C α = 0.022 wt % C ; Eutectoid composition C e = 0.77 wt % C C_e = 0.77\text{ wt}\% \text{ C} C e = 0.77 wt % C ; Cementite composition C F e 3 C = 6.70 wt % C C Fe_3C = 6.70\text{ wt}\% \text{ C} CF e 3 C = 6.70 wt % C .
Solution:
Proeutectoid Ferrite ( W α ′ W_{\alpha'} W α ′ ): Calculated using tie-line between C α = 0.022 % C_\alpha = 0.022\% C α = 0.022% and C e = 0.77 % C_e = 0.77\% C e = 0.77% : W α ′ = C e − C 0 C e − C α = 0.77 − 0.45 0.77 − 0.022 = 0.32 0.748 = 0.4278 ⟹ 42.78 % W_{\alpha'} = \frac{C_e - C_0}{C_e - C\alpha} = \frac{0.77 - 0.45}{0.77 - 0.022} = \frac{0.32}{0.748} = 0.4278 \implies 42.78\% W α ′ = C e − C α C e − C 0 = 0.77 − 0.022 0.77 − 0.45 = 0.748 0.32 = 0.4278 ⟹ 42.78%
Total Ferrite ( W α , total W_{\alpha, \text{total}} W α , total ): Calculated using full tie-line between C α = 0.022 % C_\alpha = 0.022\% C α = 0.022% and C F e 3 C = 6.70 % C Fe_3C = 6.70\% CF e 3 C = 6.70% : W α , total = C F e 3 C − C 0 C F e 3 C − C α = 6.70 − 0.45 6.70 − 0.022 = 6.25 6.678 = 0.9359 ⟹ 93.59 % W_{\alpha, \text{total}} = \frac{C Fe_3C - C_0}{C Fe_3C - C\alpha} = \frac{6.70 - 0.45}{6.70 - 0.022} = \frac{6.25}{6.678} = 0.9359 \implies 93.59\% W α , total = CF e 3 C − C α CF e 3 C − C 0 = 6.70 − 0.022 6.70 − 0.45 = 6.678 6.25 = 0.9359 ⟹ 93.59%
Pearlite ( W P W_P W P ): The pearlite fraction equals the remaining austenite fraction just above 727 ∘ C 727^\circ\text{C} 72 7 ∘ C : W P = 1 − W α ′ = 1 − 0.4278 = 0.5722 ⟹ 57.22 % W_P = 1 - W_{\alpha'} = 1 - 0.4278 = 0.5722 \implies 57.22\% W P = 1 − W α ′ = 1 − 0.4278 = 0.5722 ⟹ 57.22%
(Check via tie-line formula: W P = C 0 − C α C e − C α = 0.45 − 0.022 0.77 − 0.022 = 0.428 0.748 = 0.5722 W_P = \frac{C_0 - C_\alpha}{C_e - C_\alpha} = \frac{0.45 - 0.022}{0.77 - 0.022} = \frac{0.428}{0.748} = 0.5722 W P = C e − C α C 0 − C α = 0.77 − 0.022 0.45 − 0.022 = 0.748 0.428 = 0.5722 . Exact match!)
8. MELE Exam Tips
Tip
Critical Temperatures: A 1 = 727 ∘ C A_1 = 727^\circ\text{C} A 1 = 72 7 ∘ C (Eutectoid line), A 3 A_3 A 3 = Upper critical temp for hypoeutectoid steel, A c m A_{cm} A c m = Solvus line for hypereutectoid steel.
Cooling Medium Severity ( H H H -value): Brine ( H ≈ 2.0 H \approx 2.0 H ≈ 2.0 ) > Water ( H = 1.0 H = 1.0 H = 1.0 ) > Oil ( H ≈ 0.3 − 0.5 H \approx 0.3-0.5 H ≈ 0.3 − 0.5 ) > Air ( H ≈ 0.02 H \approx 0.02 H ≈ 0.02 ). Higher severity increases quench speed but raises cracking/warping risk.
Difference Between Hardness and Hardenability: Hardness is resistance to indentation (controlled by % Carbon \% \text{ Carbon} % Carbon ). Hardenability is the depth of hardness penetration (controlled by alloying elements like Cr, Ni, Mo \text{Cr, Ni, Mo} Cr, Ni, Mo ).