Study guide

4.4 Chain Sling Inspection, Wear & Rejection Criteria

LEEA Foundation Certificate Lifting Equipment Engineers Association, UK

Track your progress as you read

Finished sections get a check mark.

1 Introduction & Exam Overview

About the LEEA Foundation Certificate The LEEA Qualification Pathway, Diplomas & the TEAM Card

2 Legislation, Standards & Regulatory Framework

1.1 Health and Safety at Work etc. Act 1974 & Management Regulations 1.2 Provision and Use of Work Equipment Regulations 1998 (PUWER 1998) 1.3 Lifting Operations and Lifting Equipment Regulations 1998 (LOLER 1998) 1.4 Standards, Marking & Documentation 1.5 Controlling Risks, Hazard Management & the 5-Step Risk Assessment

3 Principles of Mechanics & Material Properties

2.1 Forces, Mass, Weight & Center of Gravity 2.2 Mechanical Properties: Stress, Strain & Safety Factors 2.3 WLL, SWL & Rating Concepts 2.4 Heat Treatment & Metallurgy in Lifting Equipment 2.5 Units of Measure, Symbols & Conversions 2.6 Basic Machines, Mechanical Advantage, Velocity Ratio & Efficiency 2.7 Verification, Test Machines, Calibration & NDT Methods

4 Shackles, Eyebolts & Threaded Fittings

3.1 Shackles: Types, Standards & Rating 3.2 Shackle Inspection, Safe Use & Rejection Criteria 3.3 Eyebolts & Eyenuts: Types & Angular Loading 3.4 Eyebolt Installation, Inspection & Rejection Criteria 3.5 Rigging Screws & Turnbuckles

5 Chain Slings & Components

4.1 Chain Sling Construction & Grades 4.2 Chain Components: Master Links, Hooks & Couplers 4.3 Chain Sling Marking, Certification & Safe Use 4.4 Chain Sling Inspection, Wear & Rejection Criteria

6 Wire Rope Slings & Terminations

5.1 Wire Rope Construction & Cores 5.2 Wire Rope Terminations & Assemblies 5.3 Wire Rope Sling Ratings & Safe Use 5.4 Wire Rope Sling Inspection & Discard Criteria

7 Textile Slings & Below-the-Hook Accessories

6.1 Flat Woven Webbing Slings 6.2 Roundslings & High-Performance Fiber Slings 6.3 Textile Sling Inspection, Chemical & Mechanical Damage 6.4 Plate Clamps, Beam Clamps & Below-the-Hook Lifters 6.5 Fibre Rope Slings & Natural Fibre Ropes 6.6 Crane Forks & C-Hooks

8 Manual & Powered Lifting Appliances

7.1 Manual Chain Blocks & Lever Hoists 7.2 Wire Rope Pull-Lifts, Winches & Jacks 7.3 Powered Hoists: Electric & Pneumatic 7.4 Cranes, Structures & Supporting Equipment 7.5 Mobile Cranes, Tower Cranes & Offshore Cranes 7.6 Offshore Containers, Pad Eyes & Lifting Sets

9 Rigging Calculations, Mode Factors & Complex Lifts

8.1 Uniform Load Method (ULM) for Multi-Leg Slings 8.2 Trigonometric Method for Multi-Leg Slings 8.3 Hitch Mode Factors: Choked, Basket & Wrap Hitches 8.4 Center of Gravity Off-Center & Asymmetric Load Calculations

4.4 Chain Sling Inspection, Wear & Rejection Criteria

Key Takeaways Explain This Topic AI

Chain slings must undergo pre-use visual checks before every shift and formal, documented 6-monthly Thorough Examinations by a qualified Competent Person under BS EN 818-6 and LOLER.

A chain link must be immediately rejected and removed from service if pitch stretch (elongation) exceeds 5% of the original nominal pitch or if interlink wear reduces the mean link diameter by more than 10%.

Exposure to temperatures exceeding 200°C requires WLL derating; exposure above 400°C causes microstructural damage (annealing/softening) requiring immediate destruction and scrap.

Acid pickling, hot-dip galvanizing, or exposure to acidic chemical environments causes severe hydrogen embrittlement in high-strength Grade 8 and Grade 10 alloy chains, leading to catastrophic brittle failure without prior deformation.

Last updated: August 2026

4.4 Chain Sling Inspection, Wear & Rejection Criteria

Alloy steel chain slings are subject to demanding operational environments involving friction, impact, dynamic shock, and severe abrasive wear. Over time, these operational stresses degrade structural integrity. To guarantee safety and prevent catastrophic dropped loads, chain slings must be subjected to rigorous inspection regimes backed by strict, non-negotiable rejection criteria. Inspectors and riggers must know exactly how to measure wear, detect subtle thermal or chemical damage, and apply rejection limits mandated by BS EN 818-6 and the LEEA Code of Practice .

1. Inspection Regimes: Pre-Use Checks vs. Thorough Examination

Safety compliance requires two complementary tiers of inspection:

Pre-Use Inspection (Shift Checks): Conducted before every work shift by trained riggers or crane operators. It consists of a visual and tactile check of the entire sling assembly to identify missing ID tags, damaged safety latches, severe gouges, twisted links, or obvious heat discoloration.

Periodic Thorough Examination: A statutory requirement under LOLER 1998 (Regulation 9) conducted at least every 6 months (or in accordance with an approved scheme of examination) by an independent Competent Person . This involves full cleaning (degreasing/shot blasting), detailed dimensional calipers measurement of link pitches and diameters, interlink wear checks, and Non-Destructive Testing (NDT) such as Magnetic Particle Inspection (MPI) where cracking is suspected.

2. Quantifiable Dimensional Rejection Thresholds

Dimensional degradation of chain links occurs primarily in two forms: pitch stretch (elongation) caused by overload, and interlink wear caused by articulation under abrasive conditions. DIMENSIONAL WEAR & PITCH MEASUREMENT

  • +----- Gauge Length (5 p) ------+
  • | |
  • ( link 1 )( link 2 )( link 3 )
  • ^ ^ ^
  • +--- Interlink Wear Points --+ <-- Measured with Calipers
  • (Max 10% Reduction) (Max 5% Stretch)
  • A. Pitch Stretch & Link Elongation Limit (5% Maximum)

Mechanism: When a chain sling is subjected to severe tensile overload, the individual short links undergo plastic deformation, lengthening the pitch p p p . Stretch can also accumulate over time due to interlink wear.

Rejection Threshold: Under BS EN 818-6, a chain sling must be immediately rejected if the pitch p p p of an individual link, or the gauge length across a strand of links (typically measured over 5 to 11 links), has elongated by more than 5% of the original nominal dimensions.

Calculation: p rejection = 1.05 × p nominal p_{\text{rejection}} = 1.05 \times p_{\text{nominal}} p rejection ​ = 1.05 × p nominal ​ Example: For an 8 mm 8\text{ mm} 8 mm chain with a nominal link pitch p = 24.0 mm p = 24.0 \text{ mm} p = 24.0 mm ( 3 × 8 mm 3 \times 8\text{ mm} 3 × 8 mm ), any link measuring p > 25.2 mm p > 25.2 \text{ mm} p > 25.2 mm requires total sling rejection.

B. Interlink Wear Limit (10% Maximum Diameter Reduction)

Mechanism: As adjacent chain links articulate under heavy load, mutual friction wears away the steel at the interlink contact crowns. Wear also occurs along the outer sides of links dragging across abrasive surfaces.

Rejection Threshold: Under BS EN 818-6, a chain link must be rejected if interlink wear or abrasive wear reduces the mean wire diameter at any point by more than 10% of the nominal wire diameter d d d .

Measurement Technique: Because wear can be uneven, the inspector must take two caliper measurements ( d 1 d_1 d 1 ​ and d 2 d_2 d 2 ​ ) at right angles to each other at the point of maximum wear, calculating the mean diameter: d mean = d 1 + d 2 2 d_{\text{mean}} = \frac{d_1 + d_2}{2} d mean ​ = 2 d 1 ​ + d 2 ​ ​ If d mean < 0.90 × d nominal ⟹ REJECT SLING \text{If } d_{\text{mean}} < 0.90 \times d_{\text{nominal}} \implies \text{REJECT SLING} If d mean ​ < 0.90 × d nominal ​ ⟹ REJECT SLING Example: For a 10 mm 10\text{ mm} 10 mm nominal chain, if d mean < 9.0 mm d_{\text{mean}} < 9.0 \text{ mm} d mean ​ < 9.0 mm , the sling must be scrapped.

3. Thermal Exposure, Heat Discoloration & Annealing

High temperatures dramatically alter the heat-treated micro-structure of alloy steel chain slings, softening the material and reducing tensile capacity.

Temperature Limits & Capacity Derating

Temperature Range Grade 80 (Grade T) Capacity Grade 100 (Grade V) Capacity Microstructural Effect

− 40 ∘ C -40^\circ\text{C} − 4 0 ∘ C to + 200 ∘ C +200^\circ\text{C} + 20 0 ∘ C 100 % 100\% 100% (Full WLL) 100 % 100\% 100% (Full WLL) Normal operating zone.

+ 200 ∘ C +200^\circ\text{C} + 20 0 ∘ C to + 300 ∘ C +300^\circ\text{C} + 30 0 ∘ C Derate to 90 % 90\% 90% WLL Derate to 90 % 90\% 90% WLL Slight tempering stress relaxation.

+ 300 ∘ C +300^\circ\text{C} + 30 0 ∘ C to + 380 ∘ C +380^\circ\text{C} + 38 0 ∘ C Derate to 75 % 75\% 75% WLL Derate to 60 % 60\% 60% WLL Moderate hardness loss.

+ 380 ∘ C +380^\circ\text{C} + 38 0 ∘ C to + 400 ∘ C +400^\circ\text{C} + 40 0 ∘ C Derate to 75 % 75\% 75% WLL STRICTLY PROHIBITED Severe annealing of Grade 100.

Above + 400 ∘ C +400^\circ\text{C} + 40 0 ∘ C STRICTLY PROHIBITED STRICTLY PROHIBITED Permanent Annealing: Total loss of heat treatment; chain turns brittle/soft.

Visual Indicators of Thermal Damage

Heat Discoloration: Blue, straw, or iridescent heat-tint colors on chain links indicate exposure to extreme temperature.

Weld Spatter & Arc Strikes: Electric arc strikes or weld splatter droplets on chain links cause intense localized heating followed by rapid air-quenching, creating localized zones of ultra-brittle martensite that initiate micro-cracks under load. Chain links exhibiting arc strikes must be scrapped immediately.

4. Chemical Attack, Acid Pickling & Hydrogen Embrittlement

High-strength alloy steel chains (Grade 80 and Grade 100) are highly susceptible to hydrogen embrittlement when exposed to acidic environments or electrochemical processing. HYDROGEN EMBRITTLEMENT MECHANISM

  • Acidic Fumes / Pickling Bath ==> Atomic Hydrogen (H+) Diffuses
  • into Steel Crystal Lattice
  • |
  • v
  • Trapped at Grain Boundaries
  • |
  • v
  • CATASTROPHIC BRITTLE FRACTURE
  • Under Low Load (No Necking!)
  • The Mechanism of Hydrogen Embrittlement

When high-strength quenched and tempered steel ( > 800 N/mm 2 > 800 \text{ N/mm}^2 > 800 N/mm 2 tensile strength) contacts acids (e.g., hydrochloric or sulfuric acid pickling baths), atomic hydrogen ( H + H^+ H + ) is released. Free hydrogen atoms diffuse rapidly into the steel's internal crystalline lattice, accumulating at grain boundaries and micro-voids. Under tensile stress, the trapped hydrogen creates extreme internal pressure, triggering sudden brittle fracture with zero plastic deformation or warning .

Critical Rule on Galvanizing and Acid Bath Immersion

Grade 80 and Grade 100 chain slings must NEVER be acid-pickled or hot-dip galvanized post-manufacture.

If galvanizing or specialized plating is required, it must be performed by the original chain manufacturer under tightly controlled, baking-de-embrittlement conditions.

Chain slings exposed to acidic chemical baths or heavy chemical fumes must be withdrawn from service immediately.

5. Mechanical Defects & Component Rejection Limits

In addition to chain link wear, terminal components (hooks, master links, Hammerlocks) must be evaluated against strict visual and mechanical defect criteria: HOOK REJECTION POINTS:

  • [1] Latch Damaged / Missing
  • [2] Throat Opening Stretched (> 5%)
  • [3] Tip Twisted (> 10° from plane)
  • [4] Wear in Saddle (> 10%)
  • [5] Cracks, Gouges, or Weld Spatter
  • Master Links & Couplers

Deformation: Any visible bend, twist, or distortion in a master link or coupling link body requires immediate rejection.

Gouges & Nicks: Deep transverse nicks or gouges introduce stress concentrations. Shallow longitudinal scores may be dressed out smoothly by qualified personnel using a fine file, provided the remaining material thickness is ≥ 90 % \ge 90\% ≥ 90% of nominal.

Hook Components

Throat Opening Distortion: A hook must be rejected if the throat opening (distance from tip to throat) has stretched by more than 5% of the original forged dimension.

Tip Twist: A hook must be rejected if the tip is twisted by more than 10 ∘ 10^\circ 1 0 ∘ out of the plane of the hook body.

Saddle Wear: Wear in the load-bearing saddle of the hook exceeding 10% of original thickness requires scrap.

Safety Latch Defect: Missing, bent, unseated, or non-functioning safety latches require immediate hook repair or replacement.

6. Summary Rejection Checklist for Chain Slings

Defect Type Rejection Limit / Condition Action Required

Identification Tag Missing, illegible, or incorrect grade/WLL details. REJECT — Remove from service until re-tagged by competent authority.

Link Pitch Stretch Increase in pitch p > 5 % p > 5\% p > 5% over nominal link length. REJECT — Scrap chain strand (indicates overload).

Interlink Wear Mean wire diameter d mean < 90 % d_{\text{mean}} < 90\% d mean ​ < 90% of nominal diameter ( 10 % 10\% 10% wear limit). REJECT — Scrap affected chain leg.

Thermal Damage Heat tint colors; exposure > 400 ∘ C >400^\circ\text{C} > 40 0 ∘ C (Grade 8) or > 380 ∘ C >380^\circ\text{C} > 38 0 ∘ C (Grade 10); weld arc strikes. REJECT — Scrap sling assembly.

Chemical Attack Exposure to acid pickling, severe corrosion, or hydrogen embrittlement. REJECT — Scrap sling assembly.

Nicks & Gouges Transverse cracks, deep gouges, or reduction > 10 % >10\% > 10% after dressing. REJECT — Replace damaged component/leg.

Hook Deformation Throat opening stretch > 5 % >5\% > 5% ; tip twist > 10 ∘ >10^\circ > 1 0 ∘ ; saddle wear > 10 % >10\% > 10% ; latch broken. REJECT — Replace hook or safety latch.

Loading diagram... Chain Interlink Wear & Dimensional Measurement Points